MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Milliken® Milldride® HHPA Hexahydrophthalic Anhydride
Categories: Other Engineering Material

Material Notes: Description: Hexahydrophthalic Anhydride (HHPA) is a saturated dicarboxylic anhydride and will undergo most of the reactions typical of this class of compounds. It is supplied as a white low-melting solid (38°C) which is miscible with most organic solvents. In water, it hydrolyzes to hexahydrophthalic acid.

Application Information: Milldride HHPA is a very effective curing agent for epoxy resins. It is also used in the preparation of alkyd and polyester resins where good color stability is important. HHPA cured epoxies are characterized by reduced color and improved electrical and physical properties as compared to amine-cured products. The low melting point of HHPA allows it to be easily handled and blended with liquid resins. Viscosities of the HHPA-epoxy mixtures are lower, pot life is extended in the absence of catalyst and curing reaction is less exothermic than with other hardeners. Areas of application including casting, laminating, embedding, coating, and impregnating electrical components.

Chemical Formula: C8H10O3

CAS No: 80-04-6

Information provided by Milliken®

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/cc
@Temperature 40.0 °C
Melted
Viscosity 23 cP
@Temperature 60.0 °C
Molecular Weight 154 g/mol
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 37.2 MPaCure: 24hr-150°C
 63.4 MPaCure: 200hr-150°C
 77.9 MPaCure: 4hr-150°C
Flexural Strength 46.9 MPaCure: 24hr-150°C
 121 MPaCure: 4hr-150°C
 167 MPaCure: 200hr-150°C
Compressive Strength 5.60 ksiCure: 24hr-150°C
 22.8 ksiCure: 200hr-150°C
 25.6 ksiCure: 4hr-150°C
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.6Cure: 200hr-150°C
 4.4Cure: 4hr-150°C
 10
@Temperature 175 °C
Cure: 24hr-150°C
 
Thermal PropertiesOriginal ValueComments
Solidus 35.0 °C
 
Processing PropertiesOriginal ValueComments
Pot Life 13.0 minCure: 24hr-150°C
 150 - 210 minCure: 200hr-150°C
 5760 - 7200 minCure: 4hr-150°C
 
Descriptive Properties
Color25Molten APHA
Content<0.2%Maleic Anhydride
 0.2%Hexahydrophthalic Acid
Neutralization Value710-730

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMILLIK027 / 194998

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.