MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Constellium ALPLAN® 7075 High-Strength Rolled Precision Aluminum Plate, Milled Both Sides
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: ALPLAN® 7075 precision plates combine a good dimensional stability with high mechanical strength. Both the outstanding flatness and the low roughness of the surfaces, protected by a plastic film, make surface milling by the end user superfluous. This combination of properties enables significant cost savings in machining. Applications include reference plates, machine housings, transport tables, jigs, robot arms.

Information provided by manufacturer

Key Words: EN AW-7075 T651
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.81 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 175
@Thickness 9.90 - 25.0 mm
 175
@Thickness 25.0 - 60.0 mm
 175
@Thickness 60.0 - 80.0 mm
Tensile Strength >= 495 MPa
@Thickness 60.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 525 MPa
@Thickness 50.0 - 60.0 mm
Temper T651; Standard EN 485-2
 >= 530 MPa
@Thickness 25.0 - 50.0 mm
Temper T651; Standard EN 485-2
 >= 540 MPa
@Thickness 9.90 - 12.5 mm
Temper T651; Standard EN 485-2
 >= 540 MPa
@Thickness 12.5 - 25.0 mm
Temper T651; Standard EN 485-2
 540 MPa
@Thickness 60.0 - 80.0 mm
Typical Strength
 565 MPa
@Thickness 25.0 - 60.0 mm
Typical Strength
 575 MPa
@Thickness 9.90 - 25.0 mm
Typical Strength
Tensile Strength, Yield >= 420 MPa
@Strain 0.2 %,
Thickness 60.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 440 MPa
@Strain 0.2 %,
Thickness 50.0 - 60.0 mm
Temper T651; Standard EN 485-2
 >= 460 MPa
@Strain 0.2 %,
Thickness 9.90 - 12.5 mm
Temper T651; Standard EN 485-2
 >= 460 MPa
@Strain 0.2 %,
Thickness 25.0 - 50.0 mm
Temper T651; Standard EN 485-2
 465 MPa
@Strain 0.2 %,
Thickness 60.0 - 80.0 mm
Typical Strength
 >= 470 MPa
@Strain 0.2 %,
Thickness 12.5 - 25.0 mm
Temper T651; Standard EN 485-2
 500 MPa
@Strain 0.2 %,
Thickness 25.0 - 60.0 mm
Typical Strength
 510 MPa
@Strain 0.2 %,
Thickness 9.90 - 25.0 mm
Typical Strength
Elongation at Break >= 4.0 %
@Thickness 50.0 - 60.0 mm
Temper T651; Standard EN 485-2
 >= 4.0 %
@Thickness 60.0 - 80.0 mm
Temper T651; Standard EN 485-2
 >= 5.0 %
@Thickness 25.0 - 50.0 mm
Temper T651; Standard EN 485-2
 >= 6.0 %
@Thickness 12.5 - 25.0 mm
Temper T651; Standard EN 485-2
 >= 8.0 %
@Thickness 9.90 - 12.5 mm
Temper T651; Standard EN 485-2
 9.0 %
@Thickness 60.0 - 80.0 mm
Typical Elongation
 10 %
@Thickness 9.90 - 25.0 mm
Typical Elongation
 10 %
@Thickness 25.0 - 60.0 mm
Typical Elongation
Modulus of Elasticity 72.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000480 - 0.00000590 ohm-cmTemper T651
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
Thermal Conductivity 115 - 140 W/m-KTemper T651
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 87.32 - 91.42 %as balance
Chromium, Cr 0.18 - 0.28 %
Copper, Cu 1.2 - 2.0 %
Iron, Fe <= 0.50 %
Magnesium, Mg 2.1 - 2.9 %
Manganese, Mn <= 0.30 %
Silicon, Si <= 0.40 %
Zinc, Zn 5.1 - 6.1 %
Zr+Ti <= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 7075-T6; 7075-T651
ALIMEX 7075 T651/T652 Aluminum Alloy Rolled
Alclad Aluminum 7075-T6, T651
Aluminum 7075-T73; 7075-T735x
Alclad Aluminum 7075-O

NCONS010 / 160273

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.