MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Composiflex FlexPLY™ High Performance Composite Spring, Spring Layup
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset

Material Notes: A variety of carbon/epoxy, E-glass epoxy, and high-temperature glass/epoxy springs and available for industrial equipment uses. Some examples of these types of machinery include conveyors, oscillating sanders, vibratory rollers, vibratory feeders, and more.

Spring Layup: 1 ply at 90° as 2nd layer on top and bottom of panel with the rest at 0°, i.e. 0,90,0,0,0...0,0,0,90,0.
Available thickness per ply: 0.005 in. and 0.010 in.

Mechanical property data measured on 0.25 in thick samples.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.85 g/ccCured
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 67
Tensile Strength 80.3 ksi
@Temperature 71.1 °C
ASTM D3039
 94.4 ksi
@Temperature 22.8 °C
ASTM D3039
Tensile Modulus 6.74e+6 psi
@Temperature 71.1 °C
Chord Modulus from 0.1 to 0.3%, P; ASTM D3039
 6.84e+6 psi
@Temperature 22.8 °C
Chord Modulus from 0.1 to 0.3%, P; ASTM D3039
Flexural Strength 108 ksi
@Temperature 71.1 °C
ASTM D790
 116 ksi
@Temperature 22.8 °C
ASTM D790
Flexural Modulus 4310 ksi
@Temperature 71.1 °C
ASTM D790
 4370 ksi
@Temperature 22.8 °C
ASTM D790
Compressive Strength 65.4 ksi
@Temperature 71.1 °C
ASTM D3410
 87.0 ksi
@Temperature 22.8 °C
ASTM D3410
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 4.82
@Frequency 1e+6 Hz
50% RH; ASTM D150
 4.98
@Frequency 100000 Hz
50% RH; ASTM D150
 5.17
@Frequency 1000 Hz
50% RH; ASTM D150
 5.25
@Frequency 60 Hz
50% RH; ASTM D150
Dielectric Strength 428 kV/in50% RH; ASTM D149
Dissipation Factor 0.0070
@Frequency 60 Hz
50% RH; ASTM D150
 0.0080
@Frequency 1000 Hz
50% RH; ASTM D150
 0.018
@Frequency 100000 Hz
50% RH; ASTM D150
 0.038
@Frequency 1e+6 Hz
50% RH; ASTM D150
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg 265 °FDMA, E'

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCOMPOS91 / 282295

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.