MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution PS 5410 HIPS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Impact Modified

Material Notes:
  • Good printability
  • Good environmental stress crack resistance
  • Low Gels
  • Trims Cleanly
  • Low Gloss (matte finish)

Information provided by Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ASTM D 792
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inASTM D 955
Melt Flow 3.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
3.0 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell L 5050ASTM D 785
Tensile Strength, Yield 17.2 MPa2500 psiASTM D 638
Elongation at Break 50 %50 %ASTM D 638
Tensile Modulus 1.69 GPa245 ksiASTM D 638
Flexural Strength 37.9 MPa5500 psiASTM D 790
Flexural Modulus 1.69 GPa245 ksiASTM D 790
Izod Impact, Notched 1.49 J/cm2.80 ft-lb/inASTM D 638
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 2.5
@Thickness 1.00 mm,
Frequency 1e+6 Hz
2.5
@Thickness 0.0394 in,
Frequency 1e+6 Hz
ASTM D 150
Dielectric Strength 15.7 kV/mm400 kV/inASTM D 696
 
Thermal PropertiesMetricEnglishComments
CTE, linear 90.0 µm/m-°C50.0 µin/in-°FASTM D 696
Vicat Softening Point 98.9 °C
@Load 1.02 kg
210 °F
@Load 2.25 lb
120°C/h; ASTM D 1525
 
Optical PropertiesMetricEnglishComments
Gloss 15 %15 %Specular Gloss, 60°; ASTM D 523

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
439 Ferritic Stainless Steel (UNS S43900)
INEOS Styrolution PS 454N HIPS
INEOS Styrolution PS 485N HIPS
Americas Styrenics STYRON® 649D High Heat Crystal Polystyrene
INEOS Styrolution PS 495N HIPS

PBASG1081 / 159624

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.