MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Hexcel® HexBond™ ST1480.03 NW 146g/m2 Epoxy Film Adhesive
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: HexBond™ ST1480 is a modified epoxy film adhesive. This 180°C/356°F cure film adhesive is specially designed for bonding metal-to-metal and composite-to-composite structures. Its formulation, based on epoxy resin, provides high peel strength and toughness with high sheer strength.

Features:

  • Excellent metal-to-metal peel strength and composite-to-composite bonding
  • 180°C/356°F cure
  • Service temperature from -55°C to 150°C (-67°F to 302°F)
  • Excellent moisture resistance in high humidity environments
  • Available in a wide range of film thicknesses
Applications:
  • Metal-to-metal bonding
  • Sandwich construction
  • Composite-to-composite bonding
Cure 1: 90 min at 180°C
Cure 2: 4h at 150°C

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Adhesive Bond Strength 7.10 MPa
@Temperature 150 °C
Single Lap Shear Strength Metal, 2000 hours 70°C / 158°F 85% RH, Cure 2; EN 2243-1
 7.20 MPa
@Temperature 150 °C
Single Lap Shear Strength Metal, 2000 hours 70°C / 158°F 85% RH, Cure 1; EN 2243-1
 9.90 MPa
@Temperature 180 °C
Single Lap Shear Strength Metal/Metal, Cure 1; EN 2243-1
 10.2 MPa
@Temperature 180 °C
Single Lap Shear Strength Metal/Metal, Cure 2; EN 2243-1
 14.2 MPa
@Temperature 120 °C
Single Lap Shear Strength Metal, 2000 hours 70°C / 158°F 85% RH, Cure 2; EN 2243-1
 14.2 MPa
@Temperature 80.0 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C in hydraulic fluid; EN 2243-1
 14.5 MPa
@Temperature 120 °C
Single Lap Shear Strength Metal, 2000 hours 70°C / 158°F 85% RH, Cure 1; EN 2243-1
 16.0 MPa
@Temperature 150 °C
Single Lap Shear Strength Metal/Metal, Cure 2; EN 2243-1
 16.1 MPa
@Temperature 150 °C
Single Lap Shear Strength Metal/Metal, Cure 1; EN 2243-1
 18.0 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C in hydraulic fluid; EN 2243-1
 19.1 MPa
@Temperature 80.0 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 50°C in hydraulic fluid/water mixture; EN 2243-1
 19.8 MPa
@Temperature 120 °C
Single Lap Shear Strength Metal/Metal, Cure 1; EN 2243-1
 20.0 MPa
@Temperature 120 °C
Single Lap Shear Strength Metal/Metal, Cure 2; EN 2243-1
 20.4 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 50°C in hydraulic fluid/water mixture; EN 2243-1
 21.1 MPa
@Temperature 135 °C
Single Lap Shear Strength Composite/Composite, Cure 1; AITM 1-0019
 21.2 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C / 158°F 85% RH, Cure 1; EN 2243-1
 21.2 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, Cure 2; EN 2243-1
 21.3 MPa
@Temperature -8.89 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F, Cure 1; AITM 1-0019
 21.7 MPa
@Temperature 80.0 °C
Single Lap Shear Strength Metal/Metal, 24 hours 23°C in solvent; EN 2243-1
 22.0 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, 2000 hours 70°C / 158°F 85% RH, Cure 2; EN 2243-1
 22.3 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, Cure 1; EN 2243-1
 22.8 MPa
@Temperature -8.89 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F, Cure 2; AITM 1-0019
 23.2 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Metal/Metal, 24 hours 23°C in solvent; EN 2243-1
 26.5 MPa
@Temperature 80.0 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F 85% RH, Cure 2; AITM 1-0019
 27.2 MPa
@Temperature -55.0 °C
Single Lap Shear Strength Metal/Metal, Cure 1; EN 2243-1
 28.9 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F, Cure 1; AITM 1-0019
 29.7 MPa
@Temperature 80.0 °C
Single Lap Shear Strength Composite/Composite, Cure 1; AITM 1-0019
 30.3 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F 85% RH, Cure 1; AITM 1-0019
 30.5 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Composite/Composite, 2000 hours 70°C / 158°F, Cure 2; AITM 1-0019
 33.8 MPa
@Temperature 22.8 °C
Single Lap Shear Strength Composite/Composite, Cure 1; AITM 1-0019
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg 111 °C4h at 150°C, 2000 hours 70°C / 158°F
 119 °C90 min at 180°C, 2000 hours 70°C / 158°F 85% RH
 180 °C4h at 150°C
 193 °C90 min at 180°C
 
Processing PropertiesOriginal ValueComments
Cure Time 4.00 hour
@Temperature 150 °C
 90.0 min
@Temperature 180 °C
 
Descriptive Properties
Climbing drum peel torque125 N/25mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHEXCB9274 / 322430

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.