MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Copolymer ML7689 Polycarbonate (PC) (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN ML7689 polycarbonate (PC) siloxane copolymer resin IS a high viscosity injection molding (IM) grade WITH good processability, offering opportunities FOR shorter IM CYCLE times compared TO standard PC resins. This resin offers extreme low temperature (-40 degree C) ductility. LEXAN ML7689resin IS FDA/EU FC compliant available IN OPAQUE colors ONLY AND IS an excellent candidate FOR food contact applications.

Features: High Impact Resistance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Density 1.19 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
Viscosity 6.0 cP
@Load 1.20 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
Melt Flow 6.0 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 50.0 MPa50 mm/min; ASTM D638
 60.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 56.0 MPa50 mm/min; ASTM D638
 57.0 MPa50 mm/min; ISO 527
Elongation at Break 100 %50 mm/min; ASTM D638
 120 %50 mm/min; ISO 527
Elongation at Yield 6.0 %50 mm/min; ASTM D638
 6.0 %50 mm/min; ISO 527
Tensile Modulus 2050 MPa50 mm/min; ASTM D638
 2150 MPa1 mm/min; ISO 527
Flexural Strength 85.0 MPayield, 2 mm/min; ISO 178
 92.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2250 MPa1.3 mm/min, 50 mm span; ASTM D790
 2250 MPa2 mm/min; ISO 178
Izod Impact Notched 850 JASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 72.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 72.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 139 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 128 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 124 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 146 °CRate B/120; ISO 306
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °CInjection Molding
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80410 / 288357

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.