MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Hyflon® MFA F1540 Perfluoropolymer
Categories: Polymer; Thermoplastic; Fluoropolymer

Material Notes: Hyflon® MFA is a unique family of perfluoro polymers which combine excellent mechanical characteristics to unique properties such as chemical inertness, high flexural endurance, inherent flame resistance, low surface energy and exceptional dielectric properties.

Hyflon® MFA F1540 is a high melt flow rate multi purpose resin with an exceptional stress crack resistance, continuous service temperature up to 225°C and a 13-15 x 10³ cycles flex-life (on a 0.3 mm film, ASTM D2176).

Applications: General Purpose; Wire & Cable Applications

Features: Flame Retardant; High ESCR (Stress Crack Resist.); High FlowSolvay recommends that only Color Master Batches based in MFA be used. Master Batches based on other fluoropolymers can negatively influence the superior processing and electrical performance of the resin. A list of suppliers can be obtained from your Solvay sales representative.

HEALTH SAFETY AND ENVIRONMENT
- Hyflon® MFA F1540 is a very inert polymer and it is not harmful if used and handled according to standard processing procedures. If handled inappropriately, it may release harmful toxic chemicals.
- Hyflon® MFA F1540 does not contain any RoHS or WEEE substances.

PACKAGING AND STORAGE
- The Hyflon® MFA F1540 resin is available in 25 kg (55 lbs.) and 500 kg (1102 lbs.) packaging. Though it has an indefinite shelf life, it is recommended to store it in a clean area, protected by direct sun light and possible contamination.

Extrusion notes: WIRE AND CABLE PROCESSING GUIDELINES
- As with other fluoropolymers, MFA is corrosive in the melt. Therefore all parts coming into prolonged contact with the melt should be made with corrosion resistant materials such as Hastelloy®, Inconel®, Monel® or Xaloy®. Chrome or nickel plating is not recommended since they are typically only sufficient for brief processing tests.
- Hyflon MFA F1540 is applied onto wire using tubing extrusion techniques similar to other thermoplastic materials. An overview of the temperature, tooling and equipment requirements are in the following tables.
- Many different screw designs can be used. Single-flight screws are recommended while barrier-flights should be avoided. A typical screw design consist of a long feed section, followed by a 2 to 6 flight transition and a 5 to 7 flight metering section. The addition of a block mixing section can improve the processing performance.
EQUIPMENT/TOOLING REQUIREMENTS
- Line Speed: 200 to 350 m/min (700 to 1200 ft/min)
- Draw Down Ratio: 80 to 120
- Draw Balance: 0.96 to 1.04
- Extruder L/D: 20/1 to 30/1
- Screen Pack: Breaker plate only is required.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.11 - 2.16 g/ccASTM D792
Melt Flow 8.0 - 18 g/10 min
@Load 5.00 kg,
Temperature 372 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 55 - 60ASTM D2240
Tensile Strength at Break >= 25.0 MPa50 mm/min; ASTM D638
Elongation at Break >= 300 %50 mm/min; ASTM D638
Tensile Modulus 400 - 500 MPa1.0 mm/min; ASTM D638
Izod Impact, Notched NBASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+17 ohm-cmASTM D257
Surface Resistance >= 1.00e+17 ohmASTM D257
Dielectric Constant 2.0
@Frequency 50 Hz
ASTM D150
 2.0
@Frequency 100000 Hz
ASTM D150
Dielectric Strength 35.0 - 40.0 kV/mm
@Thickness 1.00 mm
ASTM D149
Dissipation Factor <= 0.00050
@Frequency 50 Hz
ASTM D150
 <= 0.00050
@Frequency 100000 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 16.0 - 24.0 J/gDSC
CTE, linear, Parallel to Flow 120 - 200 µm/m-°CASTM D696
Specific Heat Capacity 0.900 - 1.10 J/g-°CASTM C351
Thermal Conductivity 0.200 W/m-K
@Temperature 40.0 °C
ASTM C177
Melting Point 265 - 275 °C
Crystallization Temperature 255 - 265 °CPeak; ASTM D3418
Flammability, UL94 V-0
Oxygen Index 95 %ASTM D2863
 
Processing PropertiesOriginal ValueComments
Zone 1 240 - 290 °CExtrusion
Zone 2 270 - 320 °CExtrusion
Zone 3 300 - 360 °CExtrusion
Zone 4 330 - 380 °CExtrusion
Zone 5 340 - 390 °CExtrusion
Adapter Temperature 370 - 400 °CExtrusion
Die Temperature 390 - 420 °CExtrusion
Melt Temperature 390 - 420 °CExtrusion
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
FormsPellets
ProcessingExtrusion Coating
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4247 / 280047

http://www.madehow.com/Volume-1/Tire.html

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.