MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Pressure Seal 101-55 Santoprene Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes:

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 52
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D2240
 52
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D2240
 52
@Temperature 150 °C,
Time 86400 sec
ASTM D2240
 53
@Temperature 135 °C,
Time 86400 sec
ASTM D2240
 53
@Temperature 125 °C,
Time 86400 sec
ASTM D2240
 53
@Temperature 100 °C,
Time 86400 sec
ASTM D2240
 54
@Temperature 100 °C,
Time 605000 sec
ASTM D2240
 54
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D2240
 54
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D2240
 54
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D2240
 54
@Temperature 125 °C,
Time 605000 sec
ASTM D2240
 54
@Temperature 150 °C,
Time 605000 sec
ASTM D2240
 55
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D2240
 55
@Temperature 135 °C,
Time 605000 sec
ASTM D2240
 55
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D2240
 56
@Temperature 135 °C,
Time 1.30e+6 sec
ASTM D2240
 57
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D2240
 57
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D2240
 58
@Temperature 135 °C,
Time 2.59e+6 sec
ASTM D2240
 58
@Temperature 135 °C,
Time 3.60e+6 sec
ASTM D2240
 55
@Time 5.00 sec
ASTM D2240
Tensile Strength 635 psiUnaged Control; ASTM D412
 640 psiDie C; ASTM D412
 302 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 434 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 603 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 606 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 628 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 635 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 653 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 660 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 661 psi
@Temperature 135 °C,
Time 86400 sec
ASTM D412
 669 psi
@Temperature 135 °C,
Time 1.30e+6 sec
ASTM D412
 669 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 678 psi
@Temperature 135 °C,
Time 605000 sec
ASTM D412
 679 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 681 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 686 psi
@Temperature 135 °C,
Time 2.59e+6 sec
ASTM D412
 689 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 706 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 709 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 738 psi
@Temperature 135 °C,
Time 3.60e+6 sec
ASTM D412
 763 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
Elongation at Break 369 %Unaged Control
 93 %
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 276 %
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 318 %
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 325 %
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 326 %
@Temperature 135 °C,
Time 86400 sec
ASTM D412
 350 %
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 359 %
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 362 %
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 362 %
@Temperature 135 °C,
Time 1.30e+6 sec
ASTM D412
 367 %
@Temperature 135 °C,
Time 605000 sec
ASTM D412
 369 %
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 373 %
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 379 %
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 387 %
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 391 %
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 402 %
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 408 %
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 417 %
@Temperature 135 °C,
Time 2.59e+6 sec
ASTM D412
 428 %
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 431 %
@Temperature 135 °C,
Time 3.60e+6 sec
ASTM D412
Elongation, Ultimate 330 %ASTM D412
Tensile Modulus 1.46 MPa
@Temperature 125 °C
Young's modulus; ASTM D797.89
 2.38 MPa
@Temperature 100 °C
Young's modulus; ASTM D797.89
 4.70 MPa
@Temperature 23.0 °C
Young's modulus; ASTM D797.89
100% Modulus 264 psiUnaged Control; ASTM D412
 290 psiASTM D412
 242 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 247 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 262 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 267 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 272 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 272 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 273 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 273 psi
@Temperature 135 °C,
Time 2.59e+6 sec
ASTM D412
 273 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 274 psi
@Temperature 135 °C,
Time 605000 sec
ASTM D412
 274 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 277 psi
@Temperature 135 °C,
Time 3.60e+6 sec
ASTM D412
 277 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 277 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 278 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 279 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 279 psi
@Temperature 135 °C,
Time 86400 sec
ASTM D412
 282 psi
@Temperature 135 °C,
Time 1.30e+6 sec
ASTM D412
 282 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
Flexural Modulus 7.80 MPa0.5 in/min. Secant modulus, 1%; ASTM D 790
Tear Strength 42.0 pli
@Temperature 100 °C
ASTM D624
 108 pli
@Temperature 25.0 °C
ASTM D624
Compression Set 14 %
@Temperature 25.0 °C,
Time 79200 sec
ASTM D395, Method B
 17 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395, Method B
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -76.0 °FASTM D746
 
Descriptive Properties
Tension Set0.06ASTM D412

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL254 / 318464

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.