MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Amodel® AT-1001L PPA, Unreinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), High Impact

Material Notes: Unreinforced, impact modified, lubricated

Amodel® AT-1001L is an unreinforced, impact modified polyphthalamide (PPA) resin that exhibits exceptional impact strength at temperatures ranging from room temperature to as low as -40°F (-40°C), which suggests possible applications in ski boots and hockey skates.

In addition, its chemical and wear resistance, combined with good mechanical properties, make Amodel® AT-1001L resin a prime candidate for applications such as anti-friction and wear resistant components, chemical, oil field, automotive and safety equipment.

- Natural: AT-1001 L NT

Markets/Uses: Oil & Gas / Down Hole / Sucker Rod Guides

Applications: Automotive Applications; Automotive Electronics; General Purpose; Housings; Industrial Applications; Industrial Parts; Machine/Mechanical Parts; Metal Replacement; Oil/Gas Applications

Features: Chemical Resistant; Ductile; Hot Water Moldability; Impact Modified; Low Temperature Impact Resistance; Low Warpage; Lubricated; Wear Resistant

Penetration Impact, ASTM D3763, 73°F, Maximum Load: 1100 lbs.
Penetration Impact, ASTM D3763, 73°F, Total Energy Absorbed: 40 ft-lbs.
Penetration Impact, ASTM D3763, 73°F, Energy to Maximum Load: 30 ft-lbs.
Penetration Impact, ASTM D3763, -10°F, Total Energy Absorbed: 40 ft-lbs.
Penetration Impact, ASTM D3763, -10°F, Maximum Load: 1260 lbs.
Penetration Impact, ASTM D3763, -10°F, Energy to Maximum Load: 30 ft-lbs.

Injection notes: MOLD TEMPERATURE
- If the wall is thick, lower temperatures may be used to prevent ejector pin problems.
STORAGE
- Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Amodel® processing guide.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.11 g/ccMethod A; ISO 1183
Water Absorption 0.75 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.017 - 0.022 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.019 - 0.021 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 62.1 MPaASTM D638
Elongation at Break 30 %ASTM D638
Elongation at Yield 6.0 %ASTM D638
Tensile Modulus 1900 MPaASTM D638
Flexural Strength 96.5 MPaASTM D790
Flexural Modulus 2210 MPaASTM D790
Poissons Ratio 0.35ASTM E132
Izod Impact, Notched 750 J/m
@Temperature -40.0 °C
ASTM D256
 1100 J/m
@Temperature 23.0 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
Melting Point 310 °C
Deflection Temperature at 1.8 MPa (264 psi) 120 °C
@Thickness 3.18 mm
Annealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Feed Temperature 79.0 °CInjection Hopper
Rear Barrel Temperature 304 - 318 °C
Front Barrel Temperature 316 - 329 °C
Melt Temperature 321 - 343 °CInjection
Mold Temperature >= 135 °C
Drying Temperature 110 °C
@Time 14400 sec
Moisture Content 0.030 - 0.060 %Injection
 
Descriptive Properties
AdditiveImpact Modifier; Lubricant; Mold Release
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorNatural Color
FormsPellets
ProcessingInjection Molding; Water-Heated Mold Injection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4098 / 279898

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.