MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC VALOX™ FR Resin ENH8530 Polybutylene Terephthalate + PET (PBT+PET)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); PBT + PET Blend, Glass Filled

Material Notes: VALOX ENH8530 is a 15% glass reinforced, non-chlorinated/brominated flame retardant Polybutylene Terephthalate/Polyethylene Terephthalate (PBT/PET) injection moldable grade with excellent chemical resistance. It has a UL94V0@1.5mm and 5VA@2.0mm flame rating. This is a good candidate for a variety of applications needing a sustainable FR PBT/PET solution.

Features: Chemical Resistance,Flame Retardant,Non-Chlorinated,Non-Brominated,ECO Compliant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.46 g/ccASTM D792
Density 1.46 g/ccISO 1183
Filler Content 15 %ASTM D229
Moisture Absorption 0.0200 %Injection Molding
Viscosity 145000 cPmelt; ISO 11443
 5.0 cP
@Load 1.20 kg,
Temperature 265 °C
MVR cc/10 min; ISO 1133
 11 cP
@Load 5.00 kg,
Temperature 250 °C
MVR cc/10 min; ASTM D1238
 13 cP
@Load 2.16 kg,
Temperature 265 °C
MVR cc/10 min; ISO 1133
 45 cP
@Load 5.00 kg,
Temperature 265 °C
MVR cc/10 min; ISO 1133
Melt Flow 15 g/10 min
@Load 5.00 kg,
Temperature 250 °C
ISO 1133
 20 g/10 min
@Load 2.16 kg,
Temperature 265 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 120ISO 2039-2
Ball Indentation Hardness 142 MPaH358/30; ISO 2039-1
Tensile Strength at Break 75.0 MPa5 mm/min; ASTM D638
 75.0 MPa5 mm/min; ISO 527
Tensile Strength, Yield 75.0 MPa5 mm/min; ASTM D638
 75.0 MPa5 mm/min; ISO 527
Elongation at Break 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Elongation at Yield 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Tensile Modulus 7200 MPa5 mm/min; ASTM D638
 7400 MPa1 mm/min; ISO 527
Flexural Strength 110 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
 110 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
 125 MPabreak, 2mm/min; ISO 178
 125 MPayield, 2 mm/min; ISO 178
Flexural Modulus 6000 MPa1.3 mm/min, 50 mm span; ASTM D790
 6300 MPa2 mm/min; ISO 178
Flexural Strain at Break 3.0 %2 mm/min; ISO 178
Izod Impact Notched 45.0 JASTM D256
 45.0 J
@Temperature -30.0 °C
ASTM D256
 45.0 J
@Temperature 0.000 °C
ASTM D256
Izod Impact, Unnotched 330 J/mASTM D4812
 280 J/m
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 22.0 kJ/m²80*10*4; ISO 180/1U
 20.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 23.0 kJ/m²ISO 179/2C
 20.0 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Charpy Impact, Notched 5.00 kJ/m²ISO 179/2C
 5.00 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmASTM D257
 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
ASTM D150
 3.3
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 19.0 kV/mm
@Thickness 3.20 mm
in oil; ASTM D149
 19.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 28.0 kV/mm
@Thickness 1.60 mm
in oil; ASTM D149
 28.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
 38.0 kV/mm
@Thickness 0.800 mm
in oil; ASTM D149
 38.0 kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
Dissipation Factor 0.010
@Frequency 1e+6 Hz
ASTM D150
 0.010
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 400 VIEC 60112
 400 - 600 VUL 746A
Hot Wire Ignition, HWI 15 - 30 sec
@Thickness >=0.800 mm
UL 746A
 >= 120 sec
@Thickness >=1.50 mm
UL 746A
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness >=0.800 mm
UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 31.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 46.0 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
CTE, linear, Transverse to Flow 63.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 165 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Hot Ball Pressure Test 125 °CPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 215 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 215 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 180 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 190 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 196 °CRate B/50; ISO 306
 200 °CRate B/120; ISO 306
 202 °CRate B/50; ASTM D1525
 215 °CRate A/50; ISO 306
 220 °CRate A/50; ASTM D1525
UL RTI, Electrical 130 °CUL 746B
UL RTI, Mechanical with Impact 75.0 °CUL 746B
UL RTI, Mechanical without Impact 130 °CUL 746B
Flammability, UL94 V-0
@Thickness >=1.50 mm
UL 94
 5VA
@Thickness >=2.00 mm
UL 94
Glow Wire Ignition Temperature 750 °C
@Thickness 0.800 mm
IEC 60695-2-13
 750 °C
@Thickness 1.50 mm
IEC 60695-2-13
 800 °C
@Thickness 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 850 °C
@Thickness 1.50 mm
IEC 60695-2-12
 960 °C
@Thickness 0.800 mm
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 265 - 275 °C
Zone 2 255 - 280 °C
Zone 3 260 - 280 °C
Melt Temperature 260 - 285 °CInjection Molding
Mold Temperature 60.0 - 110 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
Precipitation Temperature 40.0 - 60.0 °CHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82786 / 290733

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.