MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Copper-Nickel-Phosphorus-Tellurium alloy, UNS C19100, HR01 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: 1/4 Hard and Stress Relieved

Fabrication Properties: Excellent Suitability – Soldering; Good Suitability – Brazing, Capacity for Being Cold Worked, Capacity for Being Hot Formed; Fair Suitability – Oxyacetylene Welding, Gas Shielded Arc Welding, Coated Metal Arc Welding; Poor Suitability – Spot Weld, Seam Weld, Butt Weld

Common Fabrication Processes: Forming and Bending; Heading and Upsetting; Hot Forging and Pressing; Roll Threading and Knurling; Shearing; Swaging

Typical uses: Components; Connectors; Bolts; Nuts; Turn buckle Barrels; Bushings; Forgings; Gears; Pinions; Screw Machine Parts; Tie Rods; Welding Torch Tips; Hardware

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.323 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 84
@Thickness 25.4 mm
 85
@Thickness 6.35 mm
 85
@Thickness 12.7 mm
 90
@Thickness 9.52 mm
 95
@Thickness 3.17 mm
Tensile Strength 78.0 ksi
@Thickness 25.4 mm
 80.0 ksi
@Thickness 12.7 mm
 84.0 ksi
@Thickness 6.35 mm
 94.0 ksi
@Thickness 9.52 mm
 104 ksi
@Thickness 3.17 mm
Tensile Strength, Yield 68.0 ksi
@Thickness 25.4 mm
0.5% Ext
 70.0 ksi
@Thickness 25.4 mm
0.2% Offset
 70.0 ksi
@Thickness 12.7 mm
0.5% Ext
 73.0 ksi
@Thickness 12.7 mm
0.2% Offset
 73.0 ksi
@Thickness 6.35 mm
0.5% Ext
 75.0 ksi
@Thickness 9.52 mm
0.5% Ext
 77.0 ksi
@Thickness 6.35 mm
0.2% Offset
 77.0 ksi
@Thickness 3.17 mm
0.5% Ext
 86.0 ksi
@Thickness 9.52 mm
0.2% Offset
 92.0 ksi
@Thickness 3.17 mm
0.2% Offset
Elongation at Break 6.0 %
@Thickness 3.17 mm
 10 %
@Thickness 6.35 mm
 10 %
@Thickness 9.52 mm
 15 %
@Thickness 12.7 mm
 27 %
@Thickness 25.4 mm
Tensile Modulus 16000 ksi
Modulus of Rigidity 6000 ksi
Poissons Ratio 0.33Calculated
Fatigue Strength 33000 psi
@Thickness 25.4 mm,
# of Cycles 1.00e+8
 33000 psi
@Thickness 6.35 mm,
# of Cycles 1.00e+8
Machinability 75 %
Forgeability 65 %
Shear Strength 41.0 ksi
@Thickness 25.4 mm
 43.0 ksi
@Thickness 12.7 mm
 44.0 ksi
@Thickness 6.35 mm
 48.0 ksi
@Thickness 9.52 mm
 56.0 ksi
@Thickness 3.17 mm
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000310 ohm-cm55% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.80 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0920 BTU/lb-°F
Thermal Conductivity 145 BTU-in/hr-ft²-°F
Melting Point 1900 - 1980 °F
Solidus 1900 °F
Liquidus 1980 °F
Annealing Point 900 - 1300 °F
 
Processing PropertiesOriginal ValueComments
Solution Temperature 1300 - 1450 °F
Hot-Working Temperature 1400 - 1600 °F
Precipitation Temperature 850 °F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 97 - 98.6 %As Balance
Iron, Fe <= 0.20 %
Lead, Pb <= 0.10 %
Nickel, Ni 0.90 - 1.3 %
Phosphorus, P 0.15 - 0.35 %
Tellurium, Te 0.35 - 0.60 %
Zinc, Zn <= 0.50 %
 
Descriptive Properties
Cold Work (%)350.5 in
 750.125 in

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC19100x4 / 292879

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.