MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 101-73 Santoprene Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes:

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.980 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 73
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D2240
 73
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D2240
 73
@Temperature 100 °C,
Time 86400 sec
ASTM D2240
 73
@Temperature 100 °C,
Time 605000 sec
ASTM D2240
 73
@Temperature 150 °C,
Time 86400 sec
ASTM D2240
 74
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D2240
 74
@Temperature 125 °C,
Time 86400 sec
ASTM D2240
 75
@Temperature 125 °C,
Time 605000 sec
ASTM D2240
 75
@Temperature 150 °C,
Time 605000 sec
ASTM D2240
 76
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D2240
 76
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D2240
 78
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D2240
 79
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D2240
 80
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D2240
 83
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D2240
 73
@Time 5.00 sec
ASTM D2240
Tensile Strength 1120 psiUnaged Control; ASTM D412
 1200 psiDie C; ASTM D412
 910 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 1030 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 1050 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 1090 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 1090 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 1110 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 1110 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 1130 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 1160 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 1170 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 1240 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 1240 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 1280 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 1310 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 1330 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
Elongation at Break 430 %Unaged Control; ASTM D412
 130 %
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 280 %
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 340 %
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 360 %
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 370 %
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 380 %
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 390 %
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 390 %
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 390 %
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 400 %
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 400 %
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 400 %
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 410 %
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 410 %
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 410 %
@Temperature 100 °C,
Time 86400 sec
ASTM D412
Elongation, Ultimate 410 %ASTM D412
Tensile Modulus 1.90 MPa
@Temperature 125 °C
Young's modulus; ASTM D797.89
 5.80 MPa
@Temperature 100 °C
Young's modulus; ASTM D797.89
 16.0 MPa
@Temperature 23.0 °C
Young's modulus; ASTM D797.89
100% Modulus 450 psiUnaged Control; ASTM D412
 470 psiASTM D412
 440 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 470 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 480 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 480 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 490 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 490 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 500 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 500 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 510 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 540 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 540 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 540 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 610 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 690 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 770 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
Flexural Modulus 24.0 MPa0.5 in/min. Secant modulus, 1%; ASTM D 790
Tear Strength 76.0 pli
@Temperature 100 °C
ASTM D624
 159 pli
@Temperature 25.0 °C
ASTM D624
Compression Set 25 %
@Temperature 25.0 °C,
Time 79200 sec
ASTM D395, Method B
 33 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395, Method B
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -81.0 °FASTM D746
 
Descriptive Properties
Tension Set0.14ASTM D412

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL258 / 318468

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.