MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Mitsubishi Chemical Advanced Materials Kyron® GC100 Injection Molded Unfilled Polyetheretherketone
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: Kyron® GC100 Polyetheretherketone PEEK, unfilled injection molded shapes exhibit superior dimensional stability and stiffness, while also delivering excellent micromachinability capabilities due to their low CTE and tensile elongation. Specifically formulated for the semiconductor and electronics industry, Kyron® GC100 PEEK components are often favored as a solution for burn in and test socket applications where precision machining is required.

Vendors: TriStar Plastics Corp. provides engineering, custom fabrication and manufacturing of high-performance plastics and self-lubricating bearing materials, such as Rulon, PEEK, Torlon, CJ Composites and Ultracomp. Capabilities include component design, material selection, prototype and production, manufacturing and surface modification. Call (800) TRI-STAR (800) 874-7827 or visit or www.TStar.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.52 g/cc1.52 g/ccASTM D792
Water Absorption 0.090 %0.090 %Immersion, 24hr; ASTM D570(2)
Water Absorption at Saturation 0.44 %0.44 %ASTM D 570(2)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 100100ASTM D785
Hardness, Rockwell R 123123ASTM D785
Tensile Strength 107 MPa15500 psiASTM D638
Elongation at Break 2.5 %2.5 %ASTM D638
Tensile Modulus 7.58 GPa1100 ksiASTM D638
Flexural Strength 165 MPa24000 psiASTM D790
Flexural Modulus 7.58 GPa1100 ksiASTM D790
Compressive Strength 159 MPa23000 psiASTM D695
Izod Impact, Notched 0.37 J/cm0.70 ft-lb/inASTM D256 Type A
K (wear) Factor 1010 x 10-8 mm³/N-M500 x 10-10 in³-min/ft-lb-hrQTM 55010
Limiting Pressure Velocity 0.175 MPa-m/sec5000 psi-ft/minat 100 FPM; QTM 55007
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+12 ohm1.00e+12 ohmANSI/ESD STM 11.11
Dielectric Constant 3.39
@Frequency 1e+6 Hz
3.39
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 13.7 kV/mm347 kV/inShort Term; ASTM D149
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 33.3 µm/m-°C
@Temperature -40.0 - 150 °C
18.5 µin/in-°F
@Temperature -40.0 - 302 °F
ASTM E831
Thermal Conductivity 0.340 W/m-K2.36 BTU-in/hr-ft²-°FASTM E1530-11
Melting Point 340 °C644 °FCrystalline, Peak; ASTM D3418
Maximum Service Temperature, Air 249 °C480 °FContinuous
Deflection Temperature at 1.8 MPa (264 psi) 229 °C445 °FASTM D648
Flammability, UL94 V-0
@Thickness 3.17 mm
V-0
@Thickness 0.125 in
 
Descriptive Properties
ColorGray

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

P1SM1Ab / 290831

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.