MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Amodel® AS-4133 L PPA, 33% glass fiber
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 30% Glass Fiber Reinforced

Material Notes: 33% glass fiber, for thick-wall parts (>3mm), fast cycle time, hot-water molds, lubricated

Amodel® AS-4133 L polyphthalamide (PPA) a 33% glass reinforced, lubricated, structural grade of polyphthalamide (PPA) that offers fast cycle times and is hot water moldable. Typical applications include electrical and electronic components.

- Black: AS-4133 L BK 324
- Natural: AS-4133 L NT

Applications: Automotive Applications; Automotive Electronics; Automotive Under the Hood; Cell Phones; Electrical/Electronic Applications; General Purpose; Housings; Industrial Applications; Machine/Mechanical Parts; Metal Replacement; Power/Other Tools; Thick-walled Parts; Valves/Valve Parts

Features: Chemical Resistant; Creep Resistant; Fast Molding Cycle; Good Dimensional Stability; Good Stiffness; High Strength; Hot Water Moldability; Low Moisture Absorption; Lubricated

Injection notes: Storage:
- Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Amodel® processing guide.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.45 g/ccASTM D792
 1.45 g/ccMethod A; ISO 1183
Water Absorption 0.29 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0050 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.010 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 200 MPaASTM D638
Elongation at Break 2.5 %ASTM D638
Tensile Modulus 11700 MPaASTM D638
Flexural Yield Strength 290 MPaASTM D790
Flexural Modulus 11000 MPaASTM D790
Compressive Strength 179 MPaASTM D695
Poissons Ratio 0.41ASTM E132
Shear Strength 90.0 MPaASTM D732
Izod Impact, Notched 80.0 J/mASTM D256
Izod Impact, Unnotched 960 J/mASTM D256
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 VUL 746
High Voltage Arc-Tracking Rate, HVTR 14.0 mm/minUL 746
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 14.0 µm/m-°C
@Temperature 149 - 249 °C
ASTM E831
 22.0 µm/m-°C
@Temperature 0.000 - 90.0 °C
ASTM E831
CTE, linear, Transverse to Flow 59.0 µm/m-°C
@Temperature 0.000 - 90.0 °C
ASTM E831
 120 µm/m-°C
@Temperature 149 - 249 °C
ASTM E831
Melting Point 320 °CDSC
 320 °C
Deflection Temperature at 0.46 MPa (66 psi) 320 °C
@Thickness 3.18 mm
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 300 °C
@Thickness 3.18 mm
Annealed; ASTM D648
Flammability, UL94 HB
@Thickness 3.20 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 318 - 324 °C
Front Barrel Temperature 327 - 332 °C
Melt Temperature 329 - 343 °CInjection
Drying Temperature 120 - 135 °C
@Time 14400 sec
Moisture Content 0.030 - 0.060 %Injection
 
Descriptive Properties
AdditiveLubricant
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack; Natural Color
FormsPellets
ProcessingWater-Heated Mold Injection Molding
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4092 / 279892

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.