Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.17 g/cc | 1.17 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 64 | 64 |
| 51 @Temperature 23.0 °C, Time 252000 sec | 51 @Temperature 73.4 °F, Time 70.0 hour |
| 53 @Temperature 23.0 °C, Time 252000 sec | 53 @Temperature 73.4 °F, Time 70.0 hour |
| 55 @Temperature 100 °C, Time 252000 sec | 55 @Temperature 212 °F, Time 70.0 hour |
| 59 @Temperature 150 °C, Time 252000 sec | 59 @Temperature 302 °F, Time 70.0 hour |
| 60 @Temperature 125 °C, Time 252000 sec | 60 @Temperature 257 °F, Time 70.0 hour |
| 61 @Temperature 100 °C, Time 252000 sec | 61 @Temperature 212 °F, Time 70.0 hour |
| 64 @Temperature 125 °C, Time 252000 sec | 64 @Temperature 257 °F, Time 70.0 hour |
| 64 @Temperature 150 °C, Time 252000 sec | 64 @Temperature 302 °F, Time 70.0 hour |
| 64 @Temperature 100 °C, Time 252000 sec | 64 @Temperature 212 °F, Time 70.0 hour |
| 64 @Temperature 23.0 °C, Time 252000 sec | 64 @Temperature 73.4 °F, Time 70.0 hour |
| 64 @Temperature 100 °C, Time 252000 sec | 64 @Temperature 212 °F, Time 70.0 hour |
| 67 @Temperature 125 °C, Time 252000 sec | 67 @Temperature 257 °F, Time 70.0 hour |
| 67 @Temperature 125 °C, Time 252000 sec | 67 @Temperature 257 °F, Time 70.0 hour |
Tensile Strength | 16.4 MPa | 2380 psi |
| 5.3167 MPa @Temperature 23.0 °C, Time 252000 sec | 771.12 psi @Temperature 73.4 °F, Time 70.0 hour |
| 7.67966 MPa @Temperature 23.0 °C, Time 252000 sec | 1113.84 psi @Temperature 73.4 °F, Time 70.0 hour |
| 14.2271 MPa @Temperature 23.0 °C, Time 252000 sec | 2063.46 psi @Temperature 73.4 °F, Time 70.0 hour |
| 14.851 MPa @Temperature 125 °C, Time 252000 sec | 2153.9 psi @Temperature 257 °F, Time 70.0 hour |
| 14.9819 MPa @Temperature 150 °C, Time 252000 sec | 2172.94 psi @Temperature 302 °F, Time 70.0 hour |
| 16.656 MPa @Temperature 100 °C, Time 252000 sec | 2415.7 psi @Temperature 212 °F, Time 70.0 hour |
| 16.6885 MPa @Temperature 150 °C, Time 252000 sec | 2420.46 psi @Temperature 302 °F, Time 70.0 hour |
| 16.984 MPa @Temperature 125 °C, Time 252000 sec | 2463.3 psi @Temperature 257 °F, Time 70.0 hour |
| 17.1151 MPa @Temperature 100 °C, Time 252000 sec | 2482.34 psi @Temperature 212 °F, Time 70.0 hour |
| 18.444 MPa @Temperature 100 °C, Time 252000 sec | 2675.1 psi @Temperature 212 °F, Time 70.0 hour |
| 19.199 MPa @Temperature 125 °C, Time 252000 sec | 2784.6 psi @Temperature 257 °F, Time 70.0 hour |
| 19.199 MPa @Temperature 125 °C, Time 252000 sec | 2784.6 psi @Temperature 257 °F, Time 70.0 hour |
Elongation, Ultimate | 554 % | 554 % |
| 202.2 % @Temperature 23.0 °C, Time 252000 sec | 202.2 % @Temperature 73.4 °F, Time 70.0 hour |
| 301.93 % @Temperature 23.0 °C, Time 252000 sec | 301.93 % @Temperature 73.4 °F, Time 70.0 hour |
| 400 % @Temperature 150 °C, Time 252000 sec | 400 % @Temperature 302 °F, Time 70.0 hour |
| 434.89 % @Temperature 150 °C, Time 252000 sec | 434.89 % @Temperature 302 °F, Time 70.0 hour |
| 443.2 % @Temperature 125 °C, Time 252000 sec | 443.2 % @Temperature 257 °F, Time 70.0 hour |
| 449.8 % @Temperature 125 °C, Time 252000 sec | 449.8 % @Temperature 257 °F, Time 70.0 hour |
| 449.8 % @Temperature 125 °C, Time 252000 sec | 449.8 % @Temperature 257 °F, Time 70.0 hour |
| 476.44 % @Temperature 100 °C, Time 252000 sec | 476.44 % @Temperature 212 °F, Time 70.0 hour |
| 486.97 % @Temperature 125 °C, Time 252000 sec | 486.97 % @Temperature 257 °F, Time 70.0 hour |
| 504.1 % @Temperature 100 °C, Time 252000 sec | 504.1 % @Temperature 212 °F, Time 70.0 hour |
| 516.2 % @Temperature 23.0 °C, Time 252000 sec | 516.2 % @Temperature 73.4 °F, Time 70.0 hour |
| 592.8 % @Temperature 100 °C, Time 252000 sec | 592.8 % @Temperature 212 °F, Time 70.0 hour |
100% Modulus | 1.81 MPa | 262 psi |
Tear Strength | 35.8 kN/m | 204 pli |
| 38.7 kN/m | 221 pli |
Compression Set | 9.0 % @Temperature 100 °C, Time 79200 sec | 9.0 % @Temperature 212 °F, Time 22.0 hour |
| 11.6 % @Temperature 125 °C, Time 79200 sec | 11.6 % @Temperature 257 °F, Time 22.0 hour |
| 13.4 % @Temperature 100 °C, Time 252000 sec | 13.4 % @Temperature 212 °F, Time 70.0 hour |
| 19.9 % @Temperature 100 °C, Time 79200 sec | 19.9 % @Temperature 212 °F, Time 22.0 hour |
| 20.3 % @Temperature 150 °C, Time 79200 sec | 20.3 % @Temperature 302 °F, Time 22.0 hour |
| 22.4 % @Temperature 125 °C, Time 79200 sec | 22.4 % @Temperature 257 °F, Time 22.0 hour |
| 29.2 % @Temperature 150 °C, Time 79200 sec | 29.2 % @Temperature 302 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -42.8 °C | -45.0 °F |
Shrinkage | -5.70 % @Temperature 100 °C, Time 252000 sec | -5.70 % @Temperature 212 °F, Time 70.0 hour |
| -5.50 % @Temperature 125 °C, Time 252000 sec | -5.50 % @Temperature 257 °F, Time 70.0 hour |
| -5.50 % @Temperature 150 °C, Time 252000 sec | -5.50 % @Temperature 302 °F, Time 70.0 hour |
| 0.80 % @Temperature 23.0 °C, Time 252000 sec | 0.80 % @Temperature 73.4 °F, Time 70.0 hour |
| 4.2 % @Temperature 100 °C, Time 252000 sec | 4.2 % @Temperature 212 °F, Time 70.0 hour |
| 5.5 % @Temperature 100 °C, Time 252000 sec | 5.5 % @Temperature 212 °F, Time 70.0 hour |
| 7.6 % @Temperature 125 °C, Time 252000 sec | 7.6 % @Temperature 257 °F, Time 70.0 hour |
| 8.5 % @Temperature 150 °C, Time 252000 sec | 8.5 % @Temperature 302 °F, Time 70.0 hour |
| 27.7 % @Temperature 23.0 °C, Time 252000 sec | 27.7 % @Temperature 73.4 °F, Time 70.0 hour |
| 50.3 % @Temperature 23.0 °C, Time 252000 sec | 50.3 % @Temperature 73.4 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |
TR-10 Temperature | -30°C |