MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Daikin DAI-EL® G-7320BP Fluoroelastomer Copolymer, Bisphenol Curable Grade, 66% Fluorine Content
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: DAI-EL® G-7320BP is a bisphenol curable, gum copolymer. It handles well on open mills and is suitable for compression, transfer or injection molding, as well as extrusion or calendering. Properly compounded, DAI-EL® G-7320BP produces vulcanizates with excellent heat and compression set resistance.

Typical Applications: O-rings, seals, gaskets, extruded tubing, calendered sheet

Rheological Properties MDR 2000:
Temperature: 177°C
Frequency: 100 cpm
Strain: 0.5°
Test time: 6 min

Rheological Properties ODR:
Temperature: 177°C
Frequency: 100 cpm
Strain: 3 °
Test time: 12 min

Information provided by Daikin.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.81 g/cc1.81 g/cc
Mooney Viscosity 38
@Temperature 121 °C
38
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7373MDR 2000
 7373ODR
Tensile Strength at Break 12.9 MPa1870 psiMDR 2000
 14.0 MPa2030 psiODR
Elongation at Break 210 %210 %ODR
 220 %220 %MDR 2000
100% Modulus  5.40 MPa
@Strain 100 %
783 psi
@Strain 100 %
MDR 2000
 5.70 MPa
@Strain 100 %
827 psi
@Strain 100 %
ODR
Compression Set  17 %
@Temperature 200 °C,
Time 252000 sec
17 %
@Temperature 392 °F,
Time 70.0 hour
#214 O-ring, MDR 2000; ASTM D395 Method B
 20 %
@Temperature 200 °C,
Time 252000 sec
20 %
@Temperature 392 °F,
Time 70.0 hour
#214 O-ring, ODR; ASTM D395 Method B
 
Thermal PropertiesMetricEnglishComments
Minimum Service Temperature, Air -18.0 °C-0.400 °FLow Temperature Retraction; ASTM D1329
 
Processing PropertiesMetricEnglishComments
Cure Time 0.900 min0.0150 hourts2, scorch time, MDR 2000
 1.10 min0.0183 hourt'50, time to 50% cure, MDR 2000
 1.50 min0.0250 hourt'90, time to 90% cure, MDR 2000
 1.50 min0.0250 hourts2, scorch time, ODR
 2.40 min0.0400 hourt'50, time to 50% cure, ODR
 2.70 min0.0450 hourt'90, time to 90% cure, ODR
 5.00 min
@Temperature 177 °C
0.0833 hour
@Temperature 351 °F
Press Cure, ODR
 10.0 min
@Temperature 177 °C
0.167 hour
@Temperature 351 °F
Press Cure, MDR 2000
 1440 min
@Temperature 232 °C
24.0 hour
@Temperature 450 °F
Post Cure, MDR 2000
 1440 min
@Temperature 260 °C
24.0 hour
@Temperature 500 °F
Post Cure, ODR
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 66 %66 %
 
Descriptive Properties
ColorWhite to pale brown
MH114 dNmmaximum torque, ODR
 22.6 dNmmaximum torque, MDR 2000
ML1.3 dNmminimum torque, MDR 2000
 11 dNmminimum torque, ODR
Test Formula0.5 phrPhosphonium accelerator
 100 phrDAI-EL® G-7320BP
 2 phrBisphenol AF
 3 phrMagnesium oxide
 30 phrMT Carbon Black (N-990)
 6 phrCalcium hydroxide

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDAIJ9833 / 209904

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.