MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPV 5165N Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 5165N is a general purpose thermoplastic vulcanizate used in automotive and industrial applications. This grade is a low hardness, medium density grade exhibiting superior compression set and chemical resistance. This grade can be processed by injection molding extrusion and profile extrusion.

Availability: Asia Pacific; Europe; Latin America; North America

Additive: UV Stabilizer

Features: General Purpose; Low Hardness; Medium Density

Uses: Blending; Flexible Grips; Gaskets; General Purpose; Profiles; Seals

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion; Profile Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.950 g/ccASTM D792
Viscosity 350 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 64
@Time 5.00 sec
Extruded; ASTM D2240
 67
@Time 5.00 sec
Injection Molded; ASTM D2240
Tensile Strength, Yield 945 psiAcross Flow; ASTM D412
 876 psi
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ASTM D573
Tensile Stress at Strain 377 psi
@Strain 100 %
Across Flow; ASTM D412
 388 psi
@Strain 100 %,
Treatment Temp. 150 °C
Across Flow, Change in Air at 168 hr; ASTM D573
Elongation at Break 650 %Across Flow; ASTM D412
 572 %
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ASTM D573
Tear Strength 200 pliDie C; ASTM D624
Compression Set 29 %
@Temperature 70.0 °C,
Time 79200 sec
ASTM D395B
 40 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395B
 
Processing PropertiesOriginal ValueComments
Processing Temperature 360 - 450 °FInjection
Rear Barrel Temperature 350 - 420 °FInjection
Middle Barrel Temperature 350 - 420 °FInjection
Front Barrel Temperature 350 - 420 °FInjection
Nozzle Temperature 370 - 430 °FInjection
Zone 1 360 - 400 °FExtrusion
Zone 2 360 - 400 °FExtrusion
Zone 3 370 - 410 °FExtrusion
Zone 4 370 - 410 °FExtrusion
Die Temperature 380 - 420 °FExtrusion
Melt Temperature 380 - 420 °FExtrusion
Mold Temperature 50.0 - 150 °FInjection
Drying Temperature 180 °F
Dry Time 3.00 hour
Screw Speed 100 - 200 rpmInjection
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 3790 Thermoplastic Vulcanizate

PTEKNQ1167 / 237658

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.