MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

BASF 3D Ultrafuse® PA Fused Fillament, Conditioned
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Components: BASF Polyamide (PA) based filament for Fused Filament Fabrication.

Product Description: The key features of Ultrafuse PA are the high strength and high modulus. Furthermore, Ultrafuse PA shows a good thermal distortion stability.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³Printed Part; ISO 1183-1
Storage Temperature 15.0 - 25.0 °C59.0 - 77.0 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 17.6 MPa2550 psiZX: Upright; ISO 527
 33.2 MPa4820 psiXY: Flat; ISO 527
Elongation at Break 12.8 %12.8 %ZX: Upright; ISO 527
 143.3 %143.3 %XY: Flat; ISO 527
Modulus of Elasticity 0.334 GPa48.4 ksiYoung's, ZX: Upright; ISO 527
 0.395 GPa57.3 ksiYoung's, XY: Flat; ISO 527
Flexural Strength 17.3 MPa2510 psiZX: Upright; ISO 178
 17.7 MPa2570 psiXY: Flat; ISO 178
 18.1 MPa2630 psiXZ: On its edge; ISO 178
Flexural Modulus 0.428 GPa62.1 ksiZX: Upright; ISO 178
 0.445 GPa64.5 ksiXY: Flat; ISO 178
 0.468 GPa67.9 ksiXZ: On its edge; ISO 178
Izod Impact, Notched (ISO) 10.1 kJ/m²4.81 ft-lb/in²ZX: Upright; ISO 180
 85.4 kJ/m²40.6 ft-lb/in²XY: Flat; ISO 180
 106 kJ/m²50.4 ft-lb/in²XZ: On its edge; ISO 180
Izod Impact, Unnotched (ISO) 17.4 kJ/m²8.28 ft-lb/in²ZX: Upright; ISO 180
 NBNBXY: Flat; ISO 180
 NBNBXZ: On its edge; ISO 180
Charpy Impact Unnotched 1.34 J/cm²6.38 ft-lb/in²ZX: Upright; ISO 179-2
 NBNBXY: Flat; ISO 179-2
 NBNBXZ: On its edge; ISO 179-2
Charpy Impact, Notched 0.940 J/cm²4.47 ft-lb/in²ZX: Upright; ISO 179-2
 13.6 J/cm²64.7 ft-lb/in²XZ: On its edge; ISO 179-2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 90.0 - 120 °C194 - 248 °FBed, Bed Material: Glass + PVA / Kapton tape / PA adhesive
Nozzle Temperature 220 - 250 °C428 - 482 °F
Drying Temperature 70.0 °C158 °Fin a hot air dryer, ensure printability
 80.0 °C176 °Fin a hot air dryer, best mechanical part properties
Dry Time 4.00 - 16.0 hour4.00 - 16.0 hour
 40.0 hour40.0 hour
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
Nozzle Diameter=0.6 mm
Print speed30-60 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASF3D011 / 312252

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.