MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
Braskem FL900PP-CF Carbon Fiber Reinforced Polypropylene 3D Printing Filament
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Carbon Fiber Filled

Material Notes: FL900PP-CF is an engineering-grade composite made from 100% recycled carbon fiber (CF) and is designed to provide robust mechanical performance while maintaining a high degree of printability for complex structures. FL900PP-CF provides engineering level performance without compromising any of PP’s inherent properties which include light weight, water resistance (no drying needed), chemical resistance, and impact resistance.

Printed part properties obtained using test specimens printed in X-Y direction.

Information provided by Braskem.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.910 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 41.0 MPaASTM D638
Elongation at Break 1.3 %ASTM D638
Modulus of Elasticity 6.38 GPaASTM D638
Flexural Modulus 4512 MPaChord Modulus; ASTM D790
Charpy Impact, Notched 11.6 kJ/m²ISO 179
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 158 °CASTM D648
Vicat Softening Point 150 °C10 N; ASTM D1525
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 240 - 260 °C
 
Descriptive Properties
Bed temperature (°C)20-40Multi-purpose adhesive spray
 80PP bed adhesion solution stick
Printing speed (mm/s)35-65

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBRAS691 / 291044

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.