MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Arla MULTICLEAR® STRONG 6Wall PC Sheet
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Optical Grade

Material Notes: MULTICLEAR® STRONG 6Wall is a unique range of extruded multiwall polycarbonate sheets specifically designed to be low U-value product with increased stiffness, allowing cost saving and providing increased light transmittance due to less glazing bars required for installation. MULTICLEAR® STRONG 6Wall is a transparent or translucent sheet with one or two sides UV protection. Standard production available in thickness 8, 10 and 16 mm, in clear, opal and bronze color. Dust free knife cutting is used in all formatting operations. MULTICLEAR® STRONG 6Wall has a 10 years limited warranty against discoloration, loss of impact strength and light transmission due to weathering. Excellent fire performance: In case of fire, the sheet will melt and allow venting where heat and smoke will be let out and therefore reduce the growth of fire by flame spread. Classification B-s1,d0 according to EN 13501-1 ( Fire classification of construction products and building elements -reaction to fire tests)

Benefits: High light transmission; Outstanding bending radius; Cross structure offering increased stiffness; Excellent thermal insulation

Application: Building industry – roofing, cladding, sidewalls, conservatories, domes, skylights, sheds, carports, smoke vents, swimming pool covers, suspended ceilings, glasshouses, shopping center roofing, railway/metro station, stadia roofing and partitions; Agriculture greenhouses, lorry /tractor ports and farm/barn buildings; Packaging boxes for lamp optics, neon signs, pallet shields and protective covers for fragile items; Advertising illuminated signs and panels.

Information provided by Arla Plast.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccISO 1183
Moisture Absorption 0.150 %
@Time 86400 sec
50% RH; ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 70ISO 2039-2
Tensile Strength at Break 70.0 MPaISO 527
Tensile Strength, Yield 63.0 MPaISO 527
Elongation at Break 110 %ISO 527
Elongation at Yield 6.0 %ISO 527
Modulus of Elasticity 2.30 GPaISO 527
Flexural Modulus 2300 MPaISO 178
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
 65.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/2D
 NB
@Temperature -40.0 °C
ISO 179/2D
 
Thermal PropertiesOriginal ValueComments
CTE, linear 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
Specific Heat Capacity 0.00117 J/g-°C
Thermal Conductivity 0.210 W/m-KDIN 52612
Deflection Temperature at 0.46 MPa (66 psi) 142 °CISO 75
Deflection Temperature at 1.8 MPa (264 psi) 132 °CISO 75
Vicat Softening Point 148 °CB 50; ISO 306
 149 °CB 120; ISO 306
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.586ISO 489

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PARLA925 / 301103

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.