MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Amodel® AT-1002 HS PPA, Unreinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), High Impact

Material Notes: Unreinforced, impact modified, heat stabilized

Amodel® AT-1002 HS is a neat, toughened, heat stabilized polyphthalamide (PPA) resin that offers superior retention of properties after humid thermal aging; high impact at low temperature and better mechanical properties than many unreinforced thermoplastic polyester and nylon resins.

This material was specifically designed for automotive electrical/electronic applications such as connectors, sockets and sensors.

- Natural: AT-1002 HS NT

Markets/Uses: Automotive / Automotive E/E / Engine Sensors; Automotive / Automotive E/E / Sensors; Automotive / Automotive E/E / Wire Harness Connectors; Automotive / Fuel Systems / Fuel Flanges; Automotive / Fuel Systems / Rollover Valves

Applications: Automotive Applications; Automotive Electronics; Automotive Under the Hood; Machine/Mechanical Parts; Metal Replacement; Valves/Valve Parts

Features: Chemical Resistant; Ductile; Heat Stabilized; Hot Water Moldability; Impact Modified; Low Temperature Impact Resistance; Low Warpage; Lubricated

Injection notes: INJECTION RATE: 1 to 3 in/sec
HOLDING PRESSURE: 50% of injection pressure
STORAGE:
- Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Amodel® processing guide.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.13 g/ccMethod A; ISO 1183
Water Absorption 0.50 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.020 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.021 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 68.3 MPaISO 527-2
Tensile Strength 83.4 MPaASTM D638
Tensile Strength, Yield 75.2 MPaISO 527-2
Elongation at Break 15 %ISO 527-2
 80 %Type IV; ASTM D638
Elongation at Yield 5.0 %ISO 527-2
Tensile Modulus 2760 MPaASTM D638
 2760 MPaISO 527-2
Flexural Strength 103 MPaASTM D790
 49.6 MPa
@Temperature 100 °C
ISO 178
 79.3 MPa
@Temperature 23.0 °C
ISO 178
Flexural Modulus 2210 MPaASTM D790
 1720 MPa
@Temperature 100 °C
ISO 178
 2280 MPa
@Temperature 23.0 °C
ISO 178
Shear Strength 64.1 MPaASTM D732
Izod Impact, Notched 140 J/mASTM D256
Izod Impact, Notched (ISO) 13.0 kJ/m²Type 1, Notch A; ISO 180
Izod Impact, Unnotched (ISO) NBType 1; ISO 180
Charpy Impact Unnotched NBType 1, Edgewise; ISO 179
Charpy Impact, Notched 13.0 kJ/m²Type 1, Edgewise, Notch A; ISO 179
Dart Drop, Total Energy 54.2 JInstrumented Dart Impact; ASTM D3763
Penetration 4448Newtons; ASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.20e+16 ohm-cmASTM D257
Surface Resistance 8.00e+13 ohmASTM D257
Dielectric Constant 3.3
@Frequency 60 Hz
ASTM D150
 3.3
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 17.0 kV/mmASTM D149
Dissipation Factor 0.0040
@Frequency 60 Hz
ASTM D150
 0.016
@Frequency 1e+6 Hz
ASTM D150
Comparative Tracking Index >= 600 VASTM D3638
High Voltage Arc-Tracking Rate, HVTR 12.0 mm/minUL 746
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 78.0 µm/m-°C
@Temperature 0.000 - 100 °C
ASTM E831
 130 µm/m-°C
@Temperature 100 - 200 °C
ASTM E831
CTE, linear, Transverse to Flow 93.0 µm/m-°C
@Temperature 0.000 - 100 °C
ASTM E831
 140 µm/m-°C
@Temperature 100 - 200 °C
ASTM E831
Melting Point 315 °CPeak; ASTM D3418
 315 °CISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 163 °CAnnealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 118 °CUnannealed, Flatwise; ISO 75-2/A
 121 °CAnnealed; ASTM D648
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 304 °C
Front Barrel Temperature 324 °C
Melt Temperature 321 - 329 °CInjection
Drying Temperature 110 °C
@Time 14400 sec
Moisture Content 0.030 - 0.060 %Injection
Screw Speed 100 - 200 rpm
 
Descriptive Properties
AdditiveHeat Stabilizer; Impact Modifier; Lubricant; Mold Release
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorNatural Color
FormsPellets
ProcessingWater-Heated Mold Injection Molding
RoHS ComplianceYes
Screw Compression Ratio2.5:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4100 / 279900

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.