MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Teknor Apex Medalist® MD-12372 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: This compound is intended for use in medical and healthcare applications, particularly for extruded medical tubing and injection molding applications for medical devices.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Autoclave Sterilizable; Ethylene Oxide Sterilizable; Good Processability; High Purity; Kink Resistant; No Animal Derived Component; Radiation (Gamma) Resistant

Uses: Medical/Healthcare Applications; Pharmaceuticals

Agency Ratings: ISO 10993 Part 5; ISO 13485

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³ASTM D792
Melt Flow 1.5 g/10 min
@Load 5.00 kg,
Temperature 200 °C
1.5 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  72
@Time 5.00 sec
72
@Time 0.00139 hour
ASTM D2240
 74
@Time 1.00 sec
74
@Time 0.000278 hour
ASTM D2240
Tensile Strength at Break 16.9 MPa2450 psiASTM D412
Tensile Stress at Strain  3.07 MPa
@Strain 50 %
445 psi
@Strain 50 %
ASTM D412
 3.65 MPa
@Strain 100 %
530 psi
@Strain 100 %
ASTM D412
 5.86 MPa
@Strain 300 %
850 psi
@Strain 300 %
ASTM D412
Elongation at Break 690 %690 %ASTM D412
Tear Strength 51.9 kN/m296 pliASTM D624
Compression Set  23 %
@Temperature 22.8 °C,
Time 79200 sec
23 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 81 %
@Temperature 70.0 °C,
Time 79200 sec
81 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Processing Temperature 193 - 227 °C380 - 440 °FMelt, Injection
Rear Barrel Temperature 149 - 171 °C300 - 340 °FInjection
Middle Barrel Temperature 171 - 193 °C340 - 380 °FInjection
Front Barrel Temperature 193 - 227 °C380 - 440 °FInjection
Nozzle Temperature 193 - 227 °C380 - 440 °FInjection
Zone 1 171 - 188 °C340 - 370 °FExtrusion
Zone 2 182 - 196 °C360 - 385 °FExtrusion
Zone 3 185 - 204 °C365 - 400 °FExtrusion
Zone 5 204 - 227 °C400 - 440 °FExtrusion
Die Temperature 204 - 227 °C400 - 440 °FExtrusion
Mold Temperature 21.1 - 51.7 °C70.0 - 125 °FInjection
Back Pressure 0.345 - 1.03 MPa50.0 - 150 psiInjection
Cushion 0.356 - 2.54 cm0.140 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceTranslucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0702 / 237193

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.