MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC Valox® 359 PBT (Europe-Africa-Middle East)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: VALOX 359 is an unreinforced, flame retarded, low warpage PBT injection moulding resin.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.32 g/ccASTM D792
Density 1.31 g/ccISO 1183
Moisture Absorption 0.140 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.50 %ISO 62
Viscosity 260000 cPMelt Viscosity, 260°C, 1500 sec-1; ISO 11443
Linear Mold Shrinkage, Flow 0.011 - 0.018 cm/cmon Tensile Bar; SABIC Method
Linear Mold Shrinkage, Transverse 0.0090 - 0.018 cm/cmon Tensile Bar; SABIC Method
Melt Flow 25 g/10 min
@Load 5.00 kg,
Temperature 265 °C
ASTM D1238
 25 g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
Melt Index of Compound 12 g/10 min
@Load 5.00 kg,
Temperature 250 °C
MVR [cm^3/10 min]; ISO 1133
 22 g/10 min
@Load 5.00 kg,
Temperature 265 °C
MVR [cm^3/10 min]; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 113ISO 2039-2
Hardness, H358/30 113 MPaISO 2039-1
Tensile Strength at Break 37.0 MPaType I, 50 mm/min; ASTM D638
 40.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 50.0 MPa50 mm/min; ISO 527
 51.0 MPaType I, 50 mm/min; ASTM D638
Elongation at Break 17 %Type I, 50 mm/min; ASTM D638
 30 %50 mm/min; ISO 527
Elongation at Yield 4.0 %Type I, 50 mm/min; ASTM D638
 5.0 %50 mm/min; ISO 527
Tensile Modulus 2050 MPa50 mm/min; ASTM D638
 2050 MPa1 mm/min; ISO 527
Flexural Yield Strength 75.0 MPa2 mm/min; ISO 178
Flexural Modulus 2100 MPa2 mm/min; ISO 178
Izod Impact, Notched 390 J/mASTM D256
 120 J/m
@Temperature -30.0 °C
ASTM D256
 170 J/m
@Temperature 0.000 °C
ASTM D256
Izod Impact, Unnotched NBASTM D4812
 NB
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 20.0 kJ/m²80*10*4; ISO 180/1A
 13.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
 15.0 kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*4; ISO 180/1U
 NB
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched NBISO 179/2C
 NBEdgew 80*10*4 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/2C
Charpy Impact, Notched 20.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 20.0 kJ/m²ISO 179/2C
 14.0 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
 15.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles 6.0CS-17, 1 kg; SABIC Method
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 2.7
@Frequency 1e+6 Hz
IEC 60250
 2.7
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 16.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 26.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
 33.0 kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
Dissipation Factor 0.0020
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.010
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 VIEC 60112
 250 - 400 VUL 746A
Hot Wire Ignition, HWI >= 120 secUL 746A
High Amp Arc Ignition, HAI 15 - 30 arcsUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 100 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 100 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
CTE, linear, Transverse to Flow 110 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 110 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Thermal Conductivity 0.180 W/m-KISO 8302
Deflection Temperature at 0.46 MPa (66 psi) 110 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
 120 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 120 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 73.0 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 73.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 145 °CRate B/50; ASTM D1525
 145 °CRate B/50; ISO 306
 145 °CRate B/120; ISO 306
 200 °CRate A/50; ISO 306
 200 °CRate A/50; ASTM D1525
UL RTI, Electrical 75.0 °CUL 746B
UL RTI, Mechanical with Impact 75.0 °CUL 746B
UL RTI, Mechanical without Impact 75.0 °CUL 746B
Flammability, UL94 V-2
@Thickness 1.50 mm
UL 94
Oxygen Index 25 %ISO 4589
Glow Wire Flammability Index 850 °C
@Thickness 1.00 mm
IEC 60695-2-12
 960 °C
@Thickness 1.60 mm
IEC 60695-2-12
 
Descriptive Properties
Ball Pressure Test, 125°C +/- 2°CPASSESIEC 60695-10-2

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI55711 / 155757

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.