MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Radici RADIFLAM® S FR 100 NT PBT, Flame Retardant, Conditioned
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: Description: PA6 flame retardant injection molding grade. Halogen and phosphorus free. Natural color. Suitable for parts where fire retardancy is required. Rated V-0 at 0.4 mm according to UL-94.

Processing: Injection Molding

Delivery Form: Granules

Additives: Release agent , Flame retarding agent

Special Characteristics: Flame Retardant, Halogen-free, Heat stabilized or stable to heat, UL Listed, Railway Application

Industries: Consumer Industry Goods, Electrical and Electronical, Transportation

Regional Availability: North America, Europe, Asia Pacific, South and Central America, Near East/Africa

Information provided by Radici Group

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.17 g/cc0.0423 lb/in³ISO 1183
Water Absorption 8.0 %
@Thickness 2.00 mm
8.0 %
@Thickness 0.0787 in
Immersion at 23°C; ISO 62
Moisture Absorption 2.00 %
@Thickness 2.00 mm
2.00 %
@Thickness 0.0787 in
50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.010 cm/cm0.010 in/inMelt Temp/Mold Temp/Cavity Pressure: 270/70/60; ISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cm0.010 in/inMelt Temp/Mold Temp/Cavity Pressure: 270/70/60; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 45.0 MPa6530 psi50 mm/min; ISO 527-2/1A
Elongation at Yield 28 %28 %50 mm/min; ISO 527-2/1A
Tensile Modulus 2.45 GPa355 ksi1mm/min; ISO 527-2/1A
Charpy Impact, Notched 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cm500V; IEC 60093
Surface Resistance 1.00e+10 ohm1.00e+10 ohm500V; IEC 60093
Dielectric Strength 30.0 kV/mm762 kV/inIEC 60243-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 160 °C320 °FISO 75/2Bf
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 - 280 °C464 - 536 °F
Mold Temperature 70.0 - 80.0 °C158 - 176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PRADICI056 / 313557

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.