MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Idemitsu Kosan XAREC™ C132 Syndiotactic Polystyrene (SPS), 30% Glass-Filled
Categories: Polymer; Thermoplastic; Polystyrene (PS); Syndiotactic Polystyrene (SPS); Syndiotactic Polystyrene (SPS) with Glass or Carbon Fiber

Material Notes: Glass fiber reinforced, flame retardant HB. PS-ST-GF30.

General Xarec™ Information: XAREC boasts remarkable heat and chemical resistance, as well as superior dimensional stability, making it the preferred SPS in many fields. XAREC is used in the automobile industry for use in critical electrical parts and components. XAREC is often applied to lead-free reflow soldering to comply with current environmental regulations such as RoHS.

Information provided by Idemitsu Losan Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.25 g/ccISO 1183
Filler Content 30 %Glass
Moisture Absorption 0.0100 %
@Time 86400 sec
50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0010 - 0.0040 cm/cmIdemitsu Method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0080 cm/cmIdemitsu Method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 120 MPaISO 527
Elongation at Break 2.1 %ISO 527
Tensile Modulus 9700 MPaISO 527
Flexural Strength 185 MPaISO 178
Flexural Modulus 9.20 GPaISO 178
Izod Impact, Notched (ISO) 13.0 kJ/m²ISO 180
Izod Impact, Unnotched (ISO) 36.0 kJ/m²ISO 180
Charpy Impact Unnotched 43.0 kJ/m²ISO 179
Charpy Impact, Notched 13.0 kJ/m²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cmIEC 60093
Dielectric Constant 2.9
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 45.0 kV/mmASTM D149
Dissipation Factor <= 0.0010
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 60 - 120 secASTM D495
Comparative Tracking Index >= 600 VIEC 60112?Solution A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 18.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
TMA
CTE, linear, Transverse to Flow 39.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
TMA
Deflection Temperature at 0.46 MPa (66 psi) 265 °CISO 75B
Deflection Temperature at 1.8 MPa (264 psi) 240 °CISO 75A
UL RTI, Electrical 50.0 °CUL746B
UL RTI, Mechanical with Impact 50.0 °CUL746B
UL RTI, Mechanical without Impact 50.0 °CUL746B
Flammability, UL94 HB
@Thickness 0.750 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 - 310 °C
Mold Temperature 130 - 155 °C
Drying Temperature 120 °C
@Time 10800 - 18000 sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PIDEM138 / 249602

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.