MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Fused Quartz
Categories: Ceramic; Oxide; Silicon Oxide

Material Notes: Silicon dioxide.

Information below is typical for commercially available fused quartz used for tubing and lighting applications. A wide variation of properties is possible between specific grades.

Key Words: SiO2, Silica, Silicon Dioxide
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.20 g/cc0.0795 lb/in³
Water Absorption 0.00 %0.00 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 820820
Hardness, Mohs 5.5 - 7.05.5 - 7.0
Modulus of Elasticity 70.0 - 78.0 GPa10200 - 11300 ksi
Compressive Strength 1100 MPa160000 psi
Poissons Ratio 0.170.17
Shear Modulus 31.0 GPa4500 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+14 - 1.00e+22 ohm-cm1.00e+14 - 1.00e+22 ohm-cm
Dielectric Constant 3.7 - 6.03.7 - 6.0
 
Thermal PropertiesMetricEnglishComments
CTE, linear  0.400 µm/m-°C
@Temperature 20.0 °C
0.222 µin/in-°F
@Temperature 68.0 °F
 0.450 µm/m-°C
@Temperature 1000 °C
0.250 µin/in-°F
@Temperature 1830 °F
 0.600 µm/m-°C
@Temperature 500 °C
0.333 µin/in-°F
@Temperature 932 °F
 0.700 µm/m-°C
@Temperature 250 °C
0.389 µin/in-°F
@Temperature 482 °F
Specific Heat Capacity 0.700 J/g-°C0.167 BTU/lb-°F
 0.670 - 0.750 J/g-°C0.160 - 0.179 BTU/lb-°F
Thermal Conductivity 1.40 - 2.00 W/m-K9.72 - 13.9 BTU-in/hr-ft²-°F
Softening Point 1580 - 1730 °C2880 - 3150 °F
Annealing Point 1100 - 1215 °C2010 - 2219 °F
Strain Point 990 - 1120 °C1810 - 2050 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.461.46
Transmission, Visible >= 90 %>= 90 %
 
Descriptive Properties
ColorClear

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Quartz (SiO2)
Silicon Dioxide, SiO2 (Alpha Quartz)
96% Silica Consolidated Reconstructed Glass
Borosilicate Glass
Borosilicate Glass, Low Expansion

BQUARTZ / 288

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.