MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Overview of materials for Liquid Crystal Polymer (LCP), Unfilled
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Unfilled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Liquid Crystal Polymer (LCP), Unfilled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.38 - 2.02 g/cc0.0499 - 0.0730 lb/in³Average value: 1.65 g/cc Grade Count:29
Water Absorption 0.0100 - 0.0400 %0.0100 - 0.0400 %Average value: 0.0217 % Grade Count:12
Moisture Absorption at Equilibrium 0.0200 - 0.0400 %0.0200 - 0.0400 %Average value: 0.0350 % Grade Count:4
Moisture Vapor Transmission 0.00606 - 0.354 cc-mm/m²-24hr-atm0.0154 - 0.900 cc-mil/100 in²-24hr-atmAverage value: 0.0960 cc-mm/m²-24hr-atm Grade Count:4
Oxygen Transmission 0.0154 - 0.0472 cc-mm/m²-24hr-atm0.0390 - 0.120 cc-mil/100 in²-24hr-atmAverage value: 0.0296 cc-mm/m²-24hr-atm Grade Count:4
Maximum Moisture Content 0.01000.0100Average value: 0.0100 Grade Count:6
Linear Mold Shrinkage 0.000200 - 0.00400 cm/cm0.000200 - 0.00400 in/inAverage value: 0.000960 cm/cm Grade Count:20
Linear Mold Shrinkage, Transverse 0.00280 - 0.00900 cm/cm0.00280 - 0.00900 in/inAverage value: 0.00456 cm/cm Grade Count:19
Melt Flow 9.00 - 18.0 g/10 min9.00 - 18.0 g/10 minAverage value: 13.7 g/10 min Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 45.0 - 90.045.0 - 90.0Average value: 70.6 Grade Count:9
Tensile Strength, Ultimate 32.0 - 182 MPa4640 - 26400 psiAverage value: 126 MPa Grade Count:29
Elongation at Break 0.600 - 4.10 %0.600 - 4.10 %Average value: 2.09 % Grade Count:29
Modulus of Elasticity 7.10 - 18.0 GPa1030 - 2610 ksiAverage value: 12.0 GPa Grade Count:16
Flexural Yield Strength 56.0 - 220 MPa8120 - 31900 psiAverage value: 160 MPa Grade Count:26
Flexural Modulus 7.03 - 20.0 GPa1020 - 2900 ksiAverage value: 12.2 GPa Grade Count:27
Flexural Strain at Break 1.30 - 4.00 %1.30 - 4.00 %Average value: 2.34 % Grade Count:13
Izod Impact, Notched (ISO) 14.0 - 95.0 kJ/m²6.66 - 45.2 ft-lb/in²Average value: 68.0 kJ/m² Grade Count:3
Charpy Impact Unnotched 0.336 - 26.7 J/cm²1.60 - 127 ft-lb/in²Average value: 4.87 J/cm² Grade Count:11
Charpy Impact, Notched 0.252 - 9.50 J/cm²1.20 - 45.2 ft-lb/in²Average value: 1.80 J/cm² Grade Count:20
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 - 1.00e+17 ohm-cm1.00e+13 - 1.00e+17 ohm-cmAverage value: 1.77e+16 ohm-cm Grade Count:19
Surface Resistance 4.10e+12 - 1.00e+15 ohm4.10e+12 - 1.00e+15 ohmAverage value: 3.77e+14 ohm Grade Count:6
Dielectric Constant 2.70 - 12.02.70 - 12.0Average value: 4.23 Grade Count:20
Dielectric Strength 19.0 - 53.0 kV/mm483 - 1350 kV/inAverage value: 32.5 kV/mm Grade Count:14
Dissipation Factor 6.00e-7 - 0.03006.00e-7 - 0.0300Average value: 0.0159 Grade Count:17
Arc Resistance 47.0 - 183 sec47.0 - 183 secAverage value: 142 sec Grade Count:13
Comparative Tracking Index 100 - 275 V100 - 275 VAverage value: 166 V Grade Count:16
 
Thermal PropertiesMetricEnglishComments
CTE, linear 6.48 - 34.0 µm/m-°C
@Temperature 20.0 - 250 °C
3.60 - 18.9 µin/in-°F
@Temperature 68.0 - 482 °F
Average value: 17.5 µm/m-°C Grade Count:3
CTE, linear, Transverse to Flow 32.0 - 64.0 µm/m-°C
@Temperature 20.0 - 250 °C
17.8 - 35.6 µin/in-°F
@Temperature 68.0 - 482 °F
Average value: 48.4 µm/m-°C Grade Count:3
Thermal Conductivity 0.500 - 34.6 W/m-K3.47 - 240 BTU-in/hr-ft²-°FAverage value: 5.06 W/m-K Grade Count:5
Melting Point 212 - 350 °C414 - 662 °FAverage value: 308 °C Grade Count:11
Deflection Temperature at 0.46 MPa (66 psi) 266 - 340 °C511 - 644 °FAverage value: 291 °C Grade Count:11
Deflection Temperature at 1.8 MPa (264 psi) 105 - 340 °C221 - 644 °FAverage value: 251 °C Grade Count:29
Flammability, UL94 V-0V-0Grade Count:21
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 350 °C68.0 - 662 °FAverage value: 162 °C Grade Count:6
Nozzle Temperature 290 - 382 °C554 - 720 °FAverage value: 342 °C Grade Count:11
Die Temperature 225 - 295 °C437 - 563 °FAverage value: 265 °C Grade Count:3
Melt Temperature 185 - 382 °C365 - 720 °FAverage value: 310 °C Grade Count:17
Mold Temperature 65.6 - 177 °C150 - 351 °FAverage value: 109 °C Grade Count:14
Drying Temperature 130 - 180 °C266 - 356 °FAverage value: 152 °C Grade Count:12
Injection Pressure 50.0 - 150 MPa7250 - 21800 psiAverage value: 104 MPa Grade Count:7

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 20% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), Carbon Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 50% Glass Fiber Filled

O2240 / 77944

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.