MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

BASF Capron® HPN 9233G 33% Glass-Filled Nylon 6 (Dry)  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: Capron HPN 9233G is a 33% glass reinforced polyamide 6 injection molding compound combining exceptional strength, stiffness and high temperature performance with excellent surface aesthetics. It is one of the High Productivity Nylon series products, offering the performance characteristics of a premium glass fiber reinforced polyamide while reducing cycle time and improving surface appearance. It is also available in heat stabilized (Capron HPN 9233G HS) and/or pigmented versions.

Capron HPN 9233G is generally recommended for high performance applications such as window locks, valve bodies, chair shells, door and window hardware, connectors, switch components, relay parts, terminal blocks, power tool housings, gears, chain saws, blowers, and trimmer housings.

Data provided by Allied Signal.

Processing: Max. water content 0.12%. Product is supplied in sealed containers and drying is not required. If drying becomes necessary, a dehumidifying or desiccant dryer operating at 85°C (185 °F). Is recommended. Drying time is dependent on moisture level.

Melt Temperature: 270-295 degC (518-563 degF). Mold Temperature: 80-95 degC (176-203 degF). Injection and Packing Pressure: 35-125 bar (500-1500psi) This product can be processed over a wide range of mold temperatures; however, for applications where aesthetics critical, a mold surface temperature of 80-95 degC (176-203 degF) is required. Injection pressure controls the filling of the part and should be applied for 90% of ram travel. Packing pressure affects the final part and can be used effectively in controlling sink marks and shrinkage. It should be applied and maintained until the gate area is completely frozen off. Back pressure can be utilized to provide uniform melt consistency and reduce trapped air and gas. A maximum of 3.5 bar (50 psi) is recommended to minimize glass fiber breakage. Fast fill rates are recommended to insure uniform melt delivery to the cavity and prevent premature freezing. Surface appearance is directly affected by injection rate.

Capron® is no longer a part of the BASF standard line. The BASF nylon products have been consolidated in the Ultramid ® line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.39 g/cc0.0502 lb/in³ISO data
Water Absorption 1.1 %1.1 %24 hrs; ISO data
Moisture Absorption at Equilibrium 1.8 %1.8 %50% RH; 23°C; ISO data
Water Absorption at Saturation 6.4 %6.4 %in water; 23°C; ISO data
Linear Mold Shrinkage 0.0030 cm/cm0.0030 in/inASTM Data MD
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 185 MPa26800 psiSame value from ASTM and ISO tests; 5 mm/min.
Elongation at Break 3.0 %3.0 %ISO, 5 mm/min
 3.0 %3.0 %ASTM, 5 mm/min
Tensile Modulus 11.17 GPa1620 ksisame value from ASTM and ISO test.
Flexural Yield Strength 295 MPa42800 psiASTM Data
Flexural Modulus 8.40 GPa1220 ksiISO Value
 9.45 GPa1370 ksiASTM Value
Poissons Ratio 0.350.35ISO data
Shear Modulus 4.10 GPa595 ksicalculated
Charpy Impact, Notched 1.30 J/cm²6.19 ft-lb/in²ISO Data
 1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO data
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmISO data
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 21.0 µm/m-°C
@Temperature 20.0 °C
11.7 µin/in-°F
@Temperature 68.0 °F
ISO data
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
ISO data
Melting Point 220 °C428 °FASTM and ISO test
Deflection Temperature at 0.46 MPa (66 psi) 218 °C424 °FISO data
Deflection Temperature at 1.8 MPa (264 psi) 207 °C405 °FISO data
 207 °C405 °FASTM Data
Flammability, UL94 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 275 °C527 °FSee Materials Notes
Mold Temperature 95.0 °C203 °FSee Materials Notes
Drying Temperature 85.0 °C185 °FSee Materials Notes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NYCOA 2256 30% Glass Filled Nylon 6
BASF Capron® 8233G 33% Glass-Filled Nylon 6 (Dry)
BASF Capron® 8233G 33% Glass-Filled Nylon 6 (Conditioned)
BASF Capron® HPN 9333G Impact Modified, 33% Glass-Filled Nylon 6 (Conditioned)
BASF Capron® 5233G 33% Glass-Filled Nylon 66 (Dry)

PALD49 / 23943

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.