MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Teknor Apex Monprene® SP-14986 XRD1 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene SP-14986 XRD1 is a general purpose thermoplastic elastomer designed for a variety of consumer applications including water sports and recreating applications, requiring a soft, rubber-like feel. Monprene SP-14986 XRD1 is a high hardness, low density, lubricated grade that exhibits a high flow and is suitable for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Abrasion Resistant; Good Colorability; Good Flexibility; Good Flow; Good Tear Strength; Good Toughness; Low Density; High Hardness; UV Resistant; Sunlight Resistant

Uses: Rubber Replacement; Sporting Goods; Swimming Pools; Water Sports Equipment

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.892 g/cc0.0322 lb/in³ASTM D792
Melt Flow 5.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
5.0 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  86
@Time 5.00 sec
86
@Time 0.00139 hour
Injection Molded; ASTM D2240
 88
@Time 1.00 sec
88
@Time 0.000278 hour
Injection Molded; ASTM D2240
Tensile Strength at Break 17.2 MPa2500 psiDie C, 20 in/min, Flow; ASTM D412
 19.0 MPa2750 psiDie C, 20 in/min, Across Flow; ASTM D412
Tensile Stress at Strain  6.27 MPa
@Strain 100 %
910 psi
@Strain 100 %
Die C, 20 in/min, Flow; ASTM D412
 7.03 MPa
@Strain 100 %
1020 psi
@Strain 100 %
Die C, 20 in/min, Across Flow; ASTM D412
 7.72 MPa
@Strain 300 %
1120 psi
@Strain 300 %
Die C, 20 in/min, Flow; ASTM D412
 8.55 MPa
@Strain 300 %
1240 psi
@Strain 300 %
Die C, 20 in/min, Across Flow; ASTM D412
Elongation at Break 640 %640 %Die C, 20 in/min, Across Flow; ASTM D412
 680 %680 %Die C, 20 in/min, Flow; ASTM D412
 
Thermal PropertiesMetricEnglishComments
Oxygen Index 20 %20 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 193 - 216 °C380 - 420 °F
Middle Barrel Temperature 193 - 216 °C380 - 420 °F
Front Barrel Temperature 193 - 216 °C380 - 420 °F
Nozzle Temperature 193 - 216 °C380 - 420 °F
Melt Temperature 193 - 216 °C380 - 420 °F
Mold Temperature 15.6 - 32.2 °C60.0 - 90.0 °F
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Translucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Monprene® SP-14966 Thermoplastic Elastomer
Teknor Apex Monprene® SP-16920 XRD2 Thermoplastic Elastomer
Teknor Apex Monprene® SP-14077 Thermoplastic Elastomer
Lanxess Mesamoll® Plastic Additive
Axiall CL-6380, CL-6380J Rigid PVC, Molding

PTEKNQ0960 / 237451

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.