MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

INEOS Styrolution Novodur® HH-112 ABS
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

Material Notes: Novodur HH-112 is a high heat injection molding grade. It provides good heat resistance combined with enhanced stiffness.

Formerly sold under the Terluran® trade name. Information provided by Styrolution

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.25 %
@Temperature 23.0 °C
0.25 %
@Temperature 73.4 °F
50% RH; ISO 62
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inISO 294-4
Melt Flow 6.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
6.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 114 MPa16500 psiISO 2039-1
Tensile Strength, Yield 58.0 MPa8410 psiISO 527
Elongation at Yield 3.1 %3.1 %ISO 527
Tensile Modulus 2.70 GPa392 ksiISO 527
Flexural Strength 81.0 MPa11700 psiISO 178
Flexural Modulus 2.70 GPa392 ksiISO 178
Charpy Impact Unnotched  8.00 J/cm²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 14.0 J/cm²
@Temperature 23.0 °C
66.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched  0.500 J/cm²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Dielectric Strength 41.0 kV/mm
@Thickness 1.50 mm
1040 kV/in
@Thickness 0.0591 in
Short Time; IEC 60243-1
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 90.0 µm/m-°C50.0 µin/in-°FISO 11359
Thermal Conductivity 0.170 W/m-K1.18 BTU-in/hr-ft²-°FDIN 52612-1
Maximum Service Temperature, Air 90.0 °C194 °F
Deflection Temperature at 0.46 MPa (66 psi) 113 °C235 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 109 °C228 °FISO 75
Vicat Softening Point  112 °C
@Load 5.10 kg
234 °F
@Load 11.2 lb
50°C/h; ISO 306
 118 °C
@Load 1.02 kg
244 °F
@Load 2.25 lb
50°C/h; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 230 - 270 °C446 - 518 °FISO 294
Mold Temperature 40.0 - 60.0 °C104 - 140 °FISO 294
Injection Velocity 200 mm/sec7.87 in/secISO 294
Drying Temperature 80.0 °C
@Time 7200 - 14400 sec
176 °F
@Time 2.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese SO.F.TER Abistir® 7120/V0-UV ABS
INEOS Styrolution Novodur® H802 ABS
Elix Polymers ELIX ABS H802 Acrylonitrile Butadiene Styrene (ABS), Heat Resistant
BASF Ultraform® N2640 Z2 POM + PUR
Covestro Bayblend® T65 XF Polycarbonate + ABS

PLANX595 / 159685

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.