MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

EMS-Grivory Grilon® TSG-30/4 W PA666-GF30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, 30% Glass Fiber Reinforced

Material Notes: Product description: Grilon TSG-30/4 W is a high heat stabilized, normal viscosity PA66 + PA6 injection molding grade with 30% glass fibers, modified for parts with high thermal demands. Grilon TSG-30/4 W has the following important properties:
  • High stiffness
  • Excellent flow behavior
  • Excellent oil resistance
  • Very good processing
  • High heat ageing resistance
  • Good surface finish
Application examples are stiff injection molding parts with high resistance against heat ageing such as functional parts in the Automotive Cooling-, Heating-, and Climatic System. Part examples are charged air cooler housings and oil sump housings in the engine compartment.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³Dry; ISO 1183
Water Absorption 5.0 %5.0 %Sim. to ISO 62
Moisture Absorption 2.00 %2.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 110 MPa16000 psiConditioned; ISO 2039-1
 210 MPa30500 psiDry; ISO 2039-1
Tensile Strength at Break 125 MPa18100 psiConditioned; ISO 527-1/-2
 190 MPa27600 psiDry; ISO 527-1/-2
Elongation at Break 3.0 %3.0 %Dry; ISO 527-1/-2
 8.0 %8.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 6.00 GPa870 ksiConditioned; ISO 527-1/-2
 9.70 GPa1410 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  6.00 J/cm²
@Temperature -30.0 °C
28.6 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 6.00 J/cm²
@Temperature -30.0 °C
28.6 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 7.00 J/cm²
@Temperature 23.0 °C
33.3 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
 8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 1.30 J/cm²
@Temperature 23.0 °C
6.19 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+10 ohm-cm1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+12 ohm-cm1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 21.0 kV/mm533 kV/inConditioned; IEC 60243-1
 25.0 kV/mm635 kV/inDry; IEC 60243-1
Comparative Tracking Index 475 V475 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C11.1 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C38.9 µin/in-°FISO 11359-1/-2
Melting Point 260 °C500 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 130 - 150 °C266 - 302 °FLong Term; ISO 2578
 230 °C446 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 235 °C455 °FISO 75-1/-2
Deflection Temperature at 8.0 MPa 155 °C311 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveAir intake systems
 Automotive electr. and electronics, lighting
 Cooling and climate control
 Hydraulic systems
Electricals & ElectronicsLighting
FormGranules
Industry & Consumer goodsHeating systems
 Hydraulics & Pneumatics
 Mechanical Engineering
ProcessingInjection Molding
Special CharacteristicsImproved heat resistance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Iupiace® GN30 m-Polyphenylene Ether (m-PPE)
Domo TECHNYL® A 218G2 V30 Black 34N PA66, 30% glass fiber, DRY
BASF Ultramid® A3WG10 BK00564 50% Glass Filled PA66 (Dry)
BASF Ultradur® B 4406 G6 BKQ113 7110 30% Glass Filled PBT
EMS-Grivory Grilon® TSG-30/4 H black 9836 PA666-GF30

PGRH267 / 156976

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.