MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Overview of materials for Polyethylene Terephthalate (PET), Glass/Mineral Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Glass/Mineral Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyethylene Terephthalate (PET), Glass/Mineral Reinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.47 - 1.85 g/cc0.0531 - 0.0668 lb/in³Average value: 1.62 g/cc Grade Count:54
 1.32 - 1.424 g/cc
@Temperature 245 - 285 °C
0.0477 - 0.05145 lb/in³
@Temperature 473 - 545 °F
Average value: 1.37 g/cc Grade Count:2
Water Absorption 0.0300 - 0.830 %0.0300 - 0.830 %Average value: 0.152 % Grade Count:16
Moisture Absorption at Equilibrium 0.0500 - 0.240 %0.0500 - 0.240 %Average value: 0.146 % Grade Count:10
Linear Mold Shrinkage 0.000500 - 0.0110 cm/cm0.000500 - 0.0110 in/inAverage value: 0.00330 cm/cm Grade Count:40
Linear Mold Shrinkage, Transverse 0.00200 - 0.0100 cm/cm0.00200 - 0.0100 in/inAverage value: 0.00745 cm/cm Grade Count:26
Ash 25.0 - 35.0 %25.0 - 35.0 %Average value: 31.7 % Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 75.0 - 11575.0 - 115Average value: 92.0 Grade Count:4
Hardness, Rockwell R 109 - 120109 - 120Average value: 116 Grade Count:14
Tensile Strength, Ultimate 80.0 - 152 MPa11600 - 22000 psiAverage value: 113 MPa Grade Count:50
 45.0 - 145 MPa
@Temperature -40.0 - 120 °C
6530 - 21000 psi
@Temperature -40.0 - 248 °F
Average value: 83.3 MPa Grade Count:1
Tensile Strength, Yield 91.0 - 145 MPa13200 - 21000 psiAverage value: 114 MPa Grade Count:4
Elongation at Break 1.00 - 7.00 %1.00 - 7.00 %Average value: 2.28 % Grade Count:44
 1.60 - 8.10 %
@Temperature -40.0 - 120 °C
1.60 - 8.10 %
@Temperature -40.0 - 248 °F
Average value: 5.33 % Grade Count:1
Modulus of Elasticity 9.70 - 13.8 GPa1410 - 2000 ksiAverage value: 11.7 GPa Grade Count:16
 2.59 - 12.27 GPa
@Temperature -40.0 - 120 °C
376 - 1780 ksi
@Temperature -40.0 - 248 °F
Average value: 6.33 GPa Grade Count:1
Flexural Yield Strength 130 - 265 MPa18900 - 38400 psiAverage value: 179 MPa Grade Count:46
Flexural Modulus 6.30 - 15.5 GPa914 - 2250 ksiAverage value: 9.81 GPa Grade Count:50
Compressive Yield Strength 126 - 180 MPa18300 - 26100 psiAverage value: 148 MPa Grade Count:5
Poissons Ratio 0.330 - 0.3400.330 - 0.340Average value: 0.335 Grade Count:11
Shear Strength 49.0 - 60.0 MPa7110 - 8700 psiAverage value: 55.8 MPa Grade Count:4
Izod Impact, Notched 0.430 - 0.910 J/cm0.806 - 1.70 ft-lb/inAverage value: 0.649 J/cm Grade Count:26
Izod Impact, Unnotched 4.27 - 5.34 J/cm8.00 - 10.0 ft-lb/inAverage value: 4.85 J/cm Grade Count:6
Izod Impact, Notched (ISO) 4.00 - 7.00 kJ/m²1.90 - 3.33 ft-lb/in²Average value: 6.16 kJ/m² Grade Count:7
 5.00 - 5.00 kJ/m²
@Temperature -30.0 - -30.0 °C
2.38 - 2.38 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 5.00 kJ/m² Grade Count:1
Charpy Impact Unnotched 2.00 - 3.50 J/cm²9.52 - 16.7 ft-lb/in²Average value: 2.86 J/cm² Grade Count:11
 2.00 - 3.50 J/cm²
@Temperature -40.0 - -30.0 °C
9.52 - 16.7 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 2.67 J/cm² Grade Count:5
Charpy Impact, Notched 0.320 - 0.900 J/cm²1.52 - 4.28 ft-lb/in²Average value: 0.666 J/cm² Grade Count:25
 0.300 - 0.800 J/cm²
@Temperature -40.0 - -30.0 °C
1.43 - 3.81 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 0.509 J/cm² Grade Count:8
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 5.00e+14 - 1.00e+17 ohm-cm5.00e+14 - 1.00e+17 ohm-cmAverage value: 2.05e+16 ohm-cm Grade Count:29
Surface Resistance 1.00e+13 - 1.00e+17 ohm1.00e+13 - 1.00e+17 ohmAverage value: 4.19e+16 ohm Grade Count:24
Dielectric Constant 3.50 - 4.503.50 - 4.50Average value: 3.89 Grade Count:10
Dielectric Strength 16.2 - 50.0 kV/mm411 - 1270 kV/inAverage value: 24.7 kV/mm Grade Count:31
Dissipation Factor 0.00500 - 0.03000.00500 - 0.0300Average value: 0.0121 Grade Count:9
Arc Resistance 75.0 - 125 sec75.0 - 125 secAverage value: 94.8 sec Grade Count:4
Comparative Tracking Index 175 - 399 V175 - 399 VAverage value: 240 V Grade Count:21
 
Thermal PropertiesMetricEnglishComments
CTE, linear 15.0 - 59.4 µm/m-°C8.33 - 33.0 µin/in-°FAverage value: 22.8 µm/m-°C Grade Count:17
 6.00 - 24.0 µm/m-°C
@Temperature 55.0 - 160 °C
3.33 - 13.3 µin/in-°F
@Temperature 131 - 320 °F
Average value: 12.6 µm/m-°C Grade Count:5
CTE, linear, Transverse to Flow 30.0 - 87.0 µm/m-°C16.7 - 48.3 µin/in-°FAverage value: 58.9 µm/m-°C Grade Count:11
 84.0 - 110 µm/m-°C
@Temperature 55.0 - 160 °C
46.7 - 61.1 µin/in-°F
@Temperature 131 - 320 °F
Average value: 91.2 µm/m-°C Grade Count:5
Specific Heat Capacity 1.79 - 1.79 J/g-°C
@Temperature 285 - 285 °C
0.428 - 0.428 BTU/lb-°F
@Temperature 545 - 545 °F
Average value: 1.79 J/g-°C Grade Count:1
Thermal Conductivity 0.320 - 0.320 W/m-K
@Temperature 285 - 285 °C
2.22 - 2.22 BTU-in/hr-ft²-°F
@Temperature 545 - 545 °F
Average value: 0.320 W/m-K Grade Count:1
Melting Point 232 - 268 °C450 - 514 °FAverage value: 251 °C Grade Count:28
Maximum Service Temperature, Air 75.0 - 140 °C167 - 284 °FAverage value: 115 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 94.0 - 243 °C201 - 470 °FAverage value: 227 °C Grade Count:16
Deflection Temperature at 1.8 MPa (264 psi) 79.0 - 242 °C174 - 468 °FAverage value: 212 °C Grade Count:53
Vicat Softening Point 205 - 225 °C401 - 437 °FAverage value: 221 °C Grade Count:5
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:35
Flame Spread 22.0 - 80.0 mm/min0.866 - 3.15 in/minAverage value: 70.9 mm/min Grade Count:10
Glow Wire Test 750 - 960 °C1380 - 1760 °FAverage value: 812 °C Grade Count:6
 
Processing PropertiesMetricEnglishComments
Processing Temperature 110 - 300 °C230 - 572 °FAverage value: 246 °C Grade Count:4
Nozzle Temperature 270 - 300 °C518 - 572 °FAverage value: 286 °C Grade Count:7
Melt Temperature 255 - 304 °C491 - 579 °FAverage value: 281 °C Grade Count:30
Mold Temperature 65.0 - 140 °C149 - 284 °FAverage value: 108 °C Grade Count:30
Drying Temperature 120 - 140 °C248 - 284 °FAverage value: 122 °C Grade Count:16
Moisture Content 0.0100 - 0.0800 %0.0100 - 0.0800 %Average value: 0.0213 % Grade Count:15
Injection Pressure 50.0 - 120 MPa7250 - 17400 psiAverage value: 72.1 MPa Grade Count:6

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyethylene Terephthalate (PET), 50% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), 20% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), 30% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced

O3338 / 78204

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.