MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

ATI Wah Chang TI-3Al-2.5V
Categories: Metal; Nonferrous Metal; Titanium Alloy

Material Notes: Ti-3Al-2.5V has proved to be a sufficiently malleable material for tube manufacture. It can be cold worked by standard tube making processes, is weldable and can be strength-ended by cold working and subsequent heat treatment to a wide range of strengths and ductilities.

Information provided by ATI Wah Chang

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.48 g/cc0.162 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  490 MPa
@Temperature 249 °C
71000 psi
@Temperature 480 °F
Annealed
 565 MPa
@Temperature 149 °C
82000 psi
@Temperature 300 °F
Annealed
 621 MPa
@Temperature 23.0 °C
90000 psi
@Temperature 73.4 °F
 717 MPa
@Temperature 249 °C
104000 psi
@Temperature 480 °F
Cold Worked
 786 MPa
@Temperature 149 °C
114000 psi
@Temperature 300 °F
Cold Worked
 896 MPa
@Temperature 23.0 °C
130000 psi
@Temperature 73.4 °F
Tensile Strength, Yield  379 MPa
@Temperature 249 °C
55000 psi
@Temperature 480 °F
Annealed
 455 MPa
@Temperature 149 °C
66000 psi
@Temperature 300 °F
Annealed
 496 MPa
@Temperature 23.0 °C
72000 psi
@Temperature 73.4 °F
 586 MPa
@Temperature 249 °C
85000 psi
@Temperature 480 °F
Cold Worked
 641 MPa
@Temperature 149 °C
93000 psi
@Temperature 300 °F
Cold Worked
 758 MPa
@Temperature 23.0 °C
110000 psi
@Temperature 73.4 °F
Elongation at Break  15 %
@Temperature 250 °C
15 %
@Temperature 482 °F
in 50 mm, Cold Worked
 17 %
@Temperature 150 °C
17 %
@Temperature 302 °F
in 50 mm, Cold Worked
 19 %
@Temperature 23.0 °C
19 %
@Temperature 73.4 °F
 23 %
@Temperature 250 °C
23 %
@Temperature 482 °F
in 50 mm, Annealed
 25 %
@Temperature 150 °C
25 %
@Temperature 302 °F
in 50 mm, Annealed
 29 %
@Temperature 23.0 °C
29 %
@Temperature 73.4 °F
Modulus of Elasticity  96.53 GPa
@Temperature 788 °C
14000 ksi
@Temperature 1450 °F
 103.4 GPa
@Temperature 23.0 °C
15000 ksi
@Temperature 73.4 °F
Poissons Ratio 0.300.30
Shear Modulus 42.7 - 44.8 GPa6200 - 6500 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000126 ohm-cm0.000126 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 9.54 µm/m-°C
@Temperature 20.0 °C
5.30 µin/in-°F
@Temperature 68.0 °F
Melting Point 1700 °C3090 °F
Beta Transus 935 °C1720 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.0 %3.0 %
Titanium, Ti 94.5 %94.5 %
Vanadium, V 2.5 %2.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-3Al-2.5V (Grade 9), Alpha-Beta Anneal, Quenched
Titanium Ti-3Al-2.5V (Grade 9), alpha annealed
Titanium Ti-3Al-2.5V (Grade 9), ST 925°C, Aged 480°C (900°F)
Titanium Ti-3Al-2.5V (Grade 9), Beta-Anneal 950°C
TIMET TIMETAL® 3-2.5 Titanium Alloy (Ti-3Al-2.5V; ASTM Grade 9) Aged

NATIWC15 / 15070

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.