MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

COI Ceramics Sylramic™ S400 Silicon Carbide Ceramic Matrix Composite, Carbon
Categories: Ceramic; Carbide; Ceramic Matrix Composite

Material Notes: Description: Engineered ceramic composite structures for a broad range of industries and applications.

Reinforcing Fiber Flexibility: S400 - Carbon
Preceramic Polymer Matrix Precursors: S400 - Crystalline (SiC + Si3N4) or SiC
Physical Attributes: Dense Matrix (<5%), High Temperature Capability, Good Matrix Dominated Properties and Wear Resistance

Typical Applications: Commercial Aviation Exhaust, Military Aircraft Propulsion Exhaust, Industrial

Information from COI Ceramics, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 2.10 g/cc0.0759 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 5.52 MPa801 psiInterlaminar
 290 MPa42100 psi
Tensile Strength, Yield 98.6 MPa14300 psi
Tensile Stress at Strain  86.2 MPa
@Strain 0.1 %
12500 psi
@Strain 0.1 %
 134 MPa
@Strain 0.2 %
19500 psi
@Strain 0.2 %
 159 MPa
@Strain 0.3 %
23000 psi
@Strain 0.3 %
 207 MPa
@Strain 0.4 %
30000 psi
@Strain 0.4 %
 262 MPa
@Strain 0.5 %
38000 psi
@Strain 0.5 %
 303 MPa
@Strain 0.6 %
44000 psi
@Strain 0.6 %
Elongation at Break 0.53 %0.53 %
Tensile Modulus 110 GPa16000 ksi
Flexural Strength 241 MPa35000 psi4 point
Shear Strength 27.6 MPa4000 psiShort Beam
 
Thermal PropertiesMetricEnglishComments
CTE, linear 2.60 µm/m-°C
@Temperature 20.0 - 1200 °C
1.44 µin/in-°F
@Temperature 68.0 - 2190 °F
 
Descriptive Properties
Nominal Fiber Volume (%)40

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
COI Ceramics Sylramic™ S200 Silicon Carbide Ceramic Matrix Composite, CG Nicalon
COI Ceramics Sylramic™ S300 Silicon Carbide Ceramic Matrix Composite, SiC
Silicon Carbide, Reaction-Bonded, SiSiC
Silicon Carbide, Alpha SiC
M Cubed Technologies SSC-FG Reaction-Bonded Silicon Carbide, Fine-Grained

CCOIC006 / 122046

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.