MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 6061-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Information provided by Alcoa and the references. General 6061 characteristics and uses: Excellent joining characteristics, good acceptance of applied coatings. Combines relatively high strength, good workability, and high resistance to corrosion; widely available. The T8 and T9 tempers offer better chipping characteristics over the T6 temper.

Uses: Aircraft fittings, camera lens mounts, couplings, marines fittings and hardware, electrical fittings and connectors, decorative or misc. hardware, hinge pins, magneto parts, brake pistons, hydraulic pistons, appliance fittings, valves and valve parts.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: al6061, UNS A96061; ISO AlMg1SiCu; Aluminium 6061-O, AD-33 (Russia); AA6061-O; Al6061-O
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.70 g/cc0.0975 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 3030AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 124 MPa18000 psiAA; Typical
Tensile Strength, Yield 55.2 MPa8000 psiAA; Typical
Elongation at Break 25 %
@Thickness 1.59 mm
25 %
@Thickness 0.0625 in
AA; Typical
 30 %
@Diameter 12.7 mm
30 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Ultimate Bearing Strength 228 MPa33100 psiEdge distance/pin diameter = 2.0
Bearing Yield Strength 103 MPa14900 psiEdge distance/pin diameter = 2.0
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 62.1 MPa
@# of Cycles 5.00e+8
9000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 30 %30 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPa3770 ksiEstimated from similar Al alloys.
Shear Strength 82.7 MPa12000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000366 ohm-cm
@Temperature 20.0 °C
0.00000366 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  23.6 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 25.2 µm/m-°C
@Temperature 20.0 - 300 °C
14.0 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.896 J/g-°C0.214 BTU/lb-°F
Thermal Conductivity 180 W/m-K1250 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 582 - 651.7 °C1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 582 °C1080 °FAA; Typical
Liquidus 651.7 °C1205 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Solution Temperature 529 °C985 °F
Aging Temperature 160 °C320 °FRolled or drawn products; hold at temperature for 18 hr
 177 °C350 °FExtrusions or forgings; hold at temperature for 8 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 95.8 - 98.6 %95.8 - 98.6 %As remainder
Chromium, Cr 0.04 - 0.35 %0.04 - 0.35 %
Copper, Cu 0.15 - 0.40 %0.15 - 0.40 %
Iron, Fe <= 0.70 %<= 0.70 %
Magnesium, Mg 0.80 - 1.2 %0.80 - 1.2 %
Manganese, Mn <= 0.15 %<= 0.15 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.40 - 0.80 %0.40 - 0.80 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6061-T4; 6061-T451
Alclad Aluminum 6061-O
Aluminum 6061-T8
Alclad Aluminum 6061-T6, T651

MA6061O / 9389

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.