MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Teknor Apex Medalist® MD-50357 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Medalist MD-50357 is intended for use in medical and healthcare applications, particularly for extruded medical tubing. Medalist MD-50357 is a medium hardness, low density, clear grade designed to be a sustainable alternative to flexible PVC for medical tubing. This grade is suitable for both injection molding and extrusion.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Autoclavable; Bondability; Ethylene Oxide Sterilizable; Good Processing Stability; High Clarity; Medium Hardness; High Purity; Kink Resistant; Low Density; Low Specific Gravity; No Animal Derived Components; Radiation (Gamma) Resistant

Uses: Medical Devices; Medical/Healthcare Applications; Pharmaceuticals; Tubing

Agency Ratings: ISO 10993 Part 5; ISO 13485

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³ASTM D792
Melt Flow 9.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
9.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  58
@Time 5.00 sec
58
@Time 0.00139 hour
ASTM D2240
 60
@Time 1.00 sec
60
@Time 0.000278 hour
ASTM D2240
Tensile Strength at Break 9.17 MPa1330 psiASTM D412
Tensile Stress at Strain  1.74 MPa
@Strain 300 %
252 psi
@Strain 300 %
ASTM D412
 1.93 MPa
@Strain 50 %
280 psi
@Strain 50 %
ASTM D412
 2.31 MPa
@Strain 100 %
335 psi
@Strain 100 %
ASTM D412
Elongation at Break 750 %750 %ASTM D412
Tear Strength 131 kN/m750 pliASTM D624
Compression Set  24 %
@Temperature 22.8 °C,
Time 79200 sec
24 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 88 %
@Temperature 70.0 °C,
Time 79200 sec
88 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Processing Temperature 193 - 216 °C380 - 420 °FMelt, Injection
Rear Barrel Temperature 149 - 171 °C300 - 340 °FInjection
Middle Barrel Temperature 171 - 193 °C340 - 380 °FInjection
Front Barrel Temperature 193 - 216 °C380 - 420 °FInjection
Nozzle Temperature 193 - 216 °C380 - 420 °FInjection
Zone 1 138 - 160 °C280 - 320 °FExtrusion
Zone 2 154 - 177 °C310 - 350 °FExtrusion
Zone 3 160 - 182 °C320 - 360 °FExtrusion
Zone 4 166 - 188 °C330 - 370 °FExtrusion
Zone 5 188 - 210 °C370 - 410 °FExtrusion
Die Temperature 171 - 210 °C340 - 410 °FExtrusion
Melt Temperature 171 - 210 °C340 - 410 °FExtrusion
Mold Temperature 21.1 - 51.7 °C70.0 - 125 °FInjection
Back Pressure 0.345 - 1.03 MPa50.0 - 150 psiInjection
Cushion 0.356 - 2.54 cm0.140 - 1.00 inInjection
Screw Speed 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceClear/Transparent
 Colors Available
 Light Blue

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-17270 Thermoplastic Elastomer
Teknor Apex Medalist® MD-12362 Thermoplastic Elastomer
Teknor Apex Medalist® MD-12160H Thermoplastic Elastomer
Teknor Apex Medalist® MD-34060 Thermoplastic Elastomer
Teknor Apex Medalist® MD-32265 Thermoplastic Elastomer

PTEKNQ0742 / 237233

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.