MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ascend Performance Materials Vydyne® 64C-R Nylon 66, Extrusion Grade
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Extruded

Material Notes: Vydyne 64C-R is a medium-viscosity PA66 resin suitable for injection-molding, extrusion and compounding applications. It is available in natural color only. 64C-R resin offers high strength, rigidity and toughness over a broad range of demanding applications and good fluid resistance to a wide variety of chemicals, solvents and oils.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³DAM; ISO 1183
Moisture Absorption at Equilibrium 2.5 %2.5 %DAM to 50% RH; ISO 62
Water Absorption at Saturation 8.5 %8.5 %ISO 62
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm
@Thickness 1.00 mm
1.00e+14 ohm-cm
@Thickness 0.0394 in
DAM; IEC 60093
Dielectric Strength 23.0 kV/mm
@Thickness 1.00 mm
584 kV/in
@Thickness 0.0394 in
DAM; IEC 60243
Arc Resistance 60 - 120 sec
@Thickness 3.00 mm
60 - 120 sec
@Thickness 0.118 in
PLC 6; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
600 V
@Thickness 0.118 in
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 15 - 30 sec15 - 30 secPLC 3; UL 746
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 0.000 - 10.0 mm/min0.000 - 0.394 in/minUL 746
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 100 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
55.6 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
55.6 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 260 °C500 °FDAM; ISO 11357-3
UL RTI, Electrical  130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746
 130 °C
@Thickness 3.00 mm
266 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  75.0 °C
@Thickness 1.50 mm
167 °F
@Thickness 0.0591 in
UL 746
 75.0 °C
@Thickness 3.00 mm
167 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  85.0 °C
@Thickness 1.50 mm
185 °F
@Thickness 0.0591 in
UL 746
 85.0 °C
@Thickness 3.00 mm
185 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  V-2
@Thickness 1.50 mm
V-2
@Thickness 0.0591 in
 V-2
@Thickness 3.00 mm
V-2
@Thickness 0.118 in
Glow Wire Ignition Temperature  700 °C
@Thickness 1.50 mm
1290 °F
@Thickness 0.0591 in
IEC 60695-2-13
 700 °C
@Thickness 3.00 mm
1290 °F
@Thickness 0.118 in
IEC 60695-2-13
Glow Wire Flammability Index  800 °C
@Thickness 1.50 mm
1470 °F
@Thickness 0.0591 in
IEC 60695-2-12
 850 °C
@Thickness 3.00 mm
1560 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Zone 1 250 - 295 °C482 - 563 °FExtrusion
Zone 2 250 - 295 °C482 - 563 °FExtrusion
Zone 3 250 - 295 °C482 - 563 °FExtrusion
Zone 4 250 - 295 °C482 - 563 °FExtrusion
Zone 5 250 - 295 °C482 - 563 °FExtrusion
Die Temperature 270 - 295 °C518 - 563 °FExtrusion
Melt Temperature 270 - 295 °C518 - 563 °FExtrusion
 
Descriptive Properties
Agency RatingsASTM, D4066 PA0112
 ASTM, D6779 PA0112
 EC, 1935/2004
 EU, 10/2011
 EU, 2023/2006
AppearanceNatural Color
FeaturesChemical Resistant
 General Purpose
 Good Toughness
 High Melt Strength
 High Rigidity
 High Strength
 Medium Viscosity
 Oil Resistant
 Solvent Resistant
FormsPellets
Processing MethodOther Extrusion
RegionNorth America, Europe, Asia Pacific
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ineos Nova 5100 High Impact Polystyrene
Ineos Nova 464 High Impact Polystyrene Injection Molding Grade
Ineos Nova 4250 High Impact Polystyrene Injection Molding Grade
Celanese Nilit FRIANYL A63 S Nylon 6.6 for injection molding
Bamberger Polymers Bapolan® 6409 Polystyrene, Injection Grade

PASCE9755 / 220858

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.