MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Envalior Xytron™ G4020DW-FC PPS-GF40 Polyphenylene Sulfide
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler

Material Notes: Xytron™ offers extremely good chemical resistance, dimensional stability, intrinsic flame retardancy and high stiffness.

Features: Drinking Water Grade. 40% glass reinforced. Drinking water grade. Food contact quality. Flame retardant. Processing: Injection molding.

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.65 g/cc0.0596 lb/in³ISO 1183
Moisture Absorption 0.0400 %0.0400 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0050 cm/cm0.0050 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  50.0 MPa
@Temperature 200 °C
7250 psi
@Temperature 392 °F
ISO 527-1/-2
 65.0 MPa
@Temperature 160 °C
9430 psi
@Temperature 320 °F
ISO 527-1/-2
 100 MPa
@Temperature 120 °C
14500 psi
@Temperature 248 °F
ISO 527-1/-2
 200 MPa
@Temperature 23.0 °C
29000 psi
@Temperature 73.4 °F
ISO 527-1/-2
Elongation at Break  2.0 %
@Temperature 23.0 °C
2.0 %
@Temperature 73.4 °F
ISO 527-1/-2
 2.9 %
@Temperature 120 °C
2.9 %
@Temperature 248 °F
ISO 527-1/-2
 3.8 %
@Temperature 160 °C
3.8 %
@Temperature 320 °F
ISO 527-1/-2
 3.9 %
@Temperature 200 °C
3.9 %
@Temperature 392 °F
ISO 527-1/-2
Tensile Modulus  4.10 GPa
@Temperature 200 °C
595 ksi
@Temperature 392 °F
ISO 527-1/-2
 5.30 GPa
@Temperature 160 °C
769 ksi
@Temperature 320 °F
ISO 527-1/-2
 9.50 GPa
@Temperature 120 °C
1380 ksi
@Temperature 248 °F
ISO 527-1/-2
 15.0 GPa
@Temperature 23.0 °C
2180 ksi
@Temperature 73.4 °F
ISO 527-1/-2
Flexural Strength 280 MPa40600 psiISO 178
Flexural Modulus  4.30 GPa
@Temperature 200 °C
624 ksi
@Temperature 392 °F
ISO 178
 5.00 GPa
@Temperature 160 °C
725 ksi
@Temperature 320 °F
ISO 178
 8.20 GPa
@Temperature 120 °C
1190 ksi
@Temperature 248 °F
ISO 178
 14.0 GPa
@Temperature 23.0 °C
2030 ksi
@Temperature 73.4 °F
ISO 178
Charpy Impact Unnotched  6.00 J/cm²
@Temperature 23.0 °C
28.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
 6.20 J/cm²
@Temperature -30.0 °C
29.5 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.05 J/cm²
@Temperature 23.0 °C
5.00 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 62631-3-1
Dielectric Constant 4.0
@Frequency 5.00e+9 Hz
4.0
@Frequency 5.00e+9 Hz
IEC 60250
Dielectric Strength 22.0 kV/mm559 kV/inIEC 60243-1
Dissipation Factor 0.0055
@Frequency 5.00e+9 Hz
0.0055
@Frequency 5.00e+9 Hz
IEC 60250
Comparative Tracking Index 150 V150 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 µm/m-°C22.2 µin/in-°FISO 11359-1/-2
 110 µm/m-°C61.1 µin/in-°Fabove Tg; ISO 11359-1/-2
CTE, linear, Parallel to Flow 15.0 µm/m-°C8.33 µin/in-°FISO 11359-1/-2
 15.0 µm/m-°C8.33 µin/in-°Fabove Tg; ISO 11359-1/-2
Melting Point 280 °C536 °F10°C/min. Dry; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 265 °C509 °FISO 75-1/-2
UL RTI, Electrical 130 °C
@Thickness 0.400 mm
266 °F
@Thickness 0.0157 in
UL746B
Flammability, UL94 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
IEC 60695-11-10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDSM7954 / 291390

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.