MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECAMID 66 MO grey Nylon 66, MoS2 Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, MoS2 Filled

Material Notes:
  • improved surface hardness
  • easy to machine
  • good mechanical properties
  • good tensile strength
Target Industries:
  • conveyor technology
  • heavy duty industry
  • mining industry
  • power engineering

Information provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³
Moisture Absorption 7.50 - 8.50 %7.50 - 8.50 %saturation; ASTM D570
 0.400 %
@Time 86400 sec
0.400 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8484ASTM D 785
Hardness, Rockwell R 119119ASTM D 785
Tensile Strength at Break 84.1 MPa12200 psiASTM D 638
Tensile Strength, Yield 82.7 MPa12000 psiASTM D 638
Elongation at Break 20 %20 %ASTM D 638
Elongation at Yield 5.0 %5.0 %ASTM D 638
Modulus of Elasticity 3.45 GPa500 ksiASTM D 638
Flexural Strength 131 MPa19000 psiASTM D 790
Flexural Modulus 3.79 GPa550 ksiASTM D 790
Compressive Yield Strength 96.5 MPa
@Strain 10 %
14000 psi
@Strain 10 %
ASTM D 695
Compressive Strength 8.27 MPa
@Strain 1 %
1200 psi
@Strain 1 %
ASTM D 695
Compressive Modulus 2.01 GPa292 ksiASTM D 695
Izod Impact, Unnotched 0.587 J/cm1.10 ft-lb/inASTM D 256
K (wear) Factor 383 x 10-8 mm³/N-M190 x 10-10 in³-min/ft-lb-hrAgainst Steel, 40 psi, 50 fpm; ASTM D 3702
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D 257
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmASTM D 257
Dielectric Constant 2.5
@Frequency 60 Hz
2.5
@Frequency 60 Hz
50% RH; ASTM D 150
Dielectric Strength 11.8 kV/mm300 kV/inASTM D 149
 
Thermal PropertiesMetricEnglishComments
CTE, linear 72.0 µm/m-°C40.0 µin/in-°FASTM D 696
Specific Heat Capacity 1.67 J/g-°C0.400 BTU/lb-°F
Melting Point 255 °C491 °F
Maximum Service Temperature, Air 110 °C230 °FLong Term
 179 °C355 °FIntermittent
Deflection Temperature at 0.46 MPa (66 psi) 243 °C470 °FASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °C194 °FASTM D 648
Flammability, UL94 HBHB
 
Descriptive Properties
Colorgrey

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENSIN8170 / 319098

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.