MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger Tecatron® XP-63 Compression Molded PPS Compound, 50% Fiberglass
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 50% Glass Fiber Filler

Material Notes: Ensinger Special Polymers has over twenty different grades of TECATRON PPS available. Custom formulations can be blended to suit specific applications. Compression molding is amenable to short run production and yields products which are homogenous with low process stress.

TECATRON PPS is a highly crystalline high-temperature thermoplastic with an excellent balance of cost, temperature resistance, strength, chemical resistance and flame retardance. TECATRON PPS is often used when long-term high-temperature performance and dimensional stability are a must, even in the presence of aggressive chemicals.

Applications:

  • Fuel Injectors
  • Manifolds
  • Pumps
  • Pistons
  • Gears
  • V-Packing Gaskets
  • Bearings

Information provided by Ensinger Special Polymers, Inc.

Vendors: Ensinger Special Polymers, Inc. provides consistent, high quality compression molded stock shapes of engineering thermoplastics. Common shapes include rings, rods, plates, tubes, and discs. Large diameter rings up to 90" OD are available.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.80 g/cc0.0650 lb/in³ASTM D792
Filler Content 50 %50 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8888ASTM D2240
Tensile Strength 36.5 MPa5300 psiASTM D638
Elongation at Break 0.80 %0.80 %ASTM D638
Tensile Modulus 9.65 GPa1400 ksiASTM D638
Flexural Strength 57.9 MPa8400 psiASTM D790
Flexural Modulus 10.3 GPa1500 ksiASTM D790
Flexural Strain at Break 0.80 %0.80 %ASTM D790
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Edgetek® SF-40GF-25MN1/000 PPS (Polyphenylene Sulfide), 40% Glass Fiber and 25% Mineral Filled
Ensinger Tecatron® XP-64 Compression Molded PPS Compound, 40% Fiberglass
Mocom (ALBIS) Tedur® L 9200-1 Polyphenylene Sulfide
MOCOM (ALBIS) Tedur® P 9519 PPS, ~45% Glass Fiber (black only)
Albis Plastics Tedur® L V 9300-1 PPS, 40% Glass Fiber/Glass Bead

PENSIN942 / 140815

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.