Idemitsu Kosan Xarec® EA 522 SPS, 22% Glass Filled
Categories:
Polymer
;
Thermoplastic
;
Polystyrene (PS)
;
Syndiotactic Polystyrene (SPS)
;
Syndiotactic Polystyrene (SPS) with Glass or Carbon Fiber
Material Notes:
Crystalline Polymer, Glass Filled, Ignition Resistant, Impact Modified. Used in Electronic and Electrical applications
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.32
g/cc
0.0477
lb/in³
Filler Content
22 %
22 %
Moisture Absorption
0.010 %
0.010 %
24 hrs., 50% RH
Linear Mold Shrinkage, Flow
0.0020
-
0.0040
cm/cm
0.0020
-
0.0040
in/in
Linear Mold Shrinkage, Transverse
0.0050
-
0.0070
cm/cm
0.0050
-
0.0070
in/in
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
100
MPa
14500
psi
Elongation at Break
2.3 %
2.3 %
Tensile Modulus
8.00
GPa
1160
ksi
Flexural Yield Strength
155
MPa
22500
psi
Flexural Modulus
7.50
GPa
1090
ksi
Izod Impact, Notched (ISO)
11.0
kJ/m²
5.23
ft-lb/in²
Izod Impact, Unnotched (ISO)
34.0
kJ/m²
16.2
ft-lb/in²
Charpy Impact Unnotched
3.90
J/cm²
18.6
ft-lb/in²
Charpy Impact, Notched
1.20
J/cm²
5.71
ft-lb/in²
Electrical Properties
Metric
English
Comments
Electrical Resistivity
1.00e+16
ohm-cm
1.00e+16
ohm-cm
Dielectric Constant
3.0
3.0
Dielectric Strength
35.0
kV/mm
889
kV/in
ASTM D145
Dissipation Factor
0.0010
0.0010
IEC 60250
Arc Resistance
120
-
180
sec
120
-
180
sec
ASTM D495
Comparative Tracking Index
400
-
600
V
400
-
600
V
IEC 60112
Hot Wire Ignition, HWI
60
-
120
sec
@Thickness 1.50 mm
60
-
120
sec
@Thickness 0.0591 in
UL 746A
High Amp Arc Ignition, HAI
>=
120
arcs
@Thickness 1.50 mm
>=
120
arcs
@Thickness 0.0591 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR
0.000
-
10.0
mm/min
0.000
-
0.394
in/min
UL746A
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
24.0
µm/m-°C
@Temperature -30.0 - 30.0 °C
13.3
µin/in-°F
@Temperature -22.0 - 86.0 °F
CTE, linear, Transverse to Flow
53.0
µm/m-°C
29.4
µin/in-°F
Deflection Temperature at 0.46 MPa (66 psi)
265
°C
509
°F
Deflection Temperature at 1.8 MPa (264 psi)
230
°C
446
°F
UL RTI, Electrical
125
°C
257
°F
UL746B
UL RTI, Mechanical with Impact
120
°C
248
°F
UL746B
UL RTI, Mechanical without Impact
120
°C
248
°F
UL746B
Flammability, UL94
V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
5VA
@Thickness 2.30 mm
5VA
@Thickness 0.0906 in
Processing Properties
Metric
English
Comments
Melt Temperature
280
-
310
°C
536
-
590
°F
Mold Temperature
50.0
-
80.0
°C
122
-
176
°F
130
-
155
°C
266
-
311
°F
For optimal surface finish
Descriptive Properties
Comments
Improved tensile elongation
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Idemitsu Kosan Xarec® WA 210 SPS, 20% Glass Filled
Idemitsu Kosan Xarec® WA 204 SPS, 20% Glass Filled
Idemitsu Kosan Xarec® WA 552 SPS, 30% Glass Filled
Idemitsu Kosan Xarec® N WA 7020 SPS, 20% Glass Filled
Celanese ZENITE 6130LX LCP, 30% Glass Reinforced
PIDEM101 / 171611
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.