MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

EVALCA EVAL® LC-H101BD Ethylene Vinyl Alcohol Copolymer Resin  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Alcohol (EVOH)

Material Notes: 38 mol % Ethylene.

Data provided by EVALCA. Applications: Blown film. EVOH is used in packaging applications because of its outstanding gas barrier properties.

EVAL™ is now produced as a part of the Kuraray product line.

Key Words: Ethylene Vinylalcohol
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.17 g/cc0.0423 lb/in³ASTM D1505
Moisture Vapor Transmission 0.820 cc-mm/m²-24hr-atm2.08 cc-mil/100 in²-24hr-atm40°C, 90% RH
Oxygen Transmission 0.0140 cc-mm/m²-24hr-atm0.0356 cc-mil/100 in²-24hr-atm20°C; 65% RH; Permeability increases significantly at higher moisture content.
Melt Flow  1.6 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.6 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 3.8 g/10 min
@Load 2.16 kg,
Temperature 210 °C
3.8 g/10 min
@Load 4.76 lb,
Temperature 410 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9595ASTM D785
Tensile Strength, Yield 67.0 MPa9720 psi10%/min. ASTM D638
Film Elongation at Break, MD 250 %250 %Orientation not specified; ASTM D882
Elongation at Yield 6.0 %6.0 %10%/min. ASTM D638
Modulus of Elasticity 2.40 GPa348 ksiYoungs Modulus, ASTM D638, 10%/min.
Flexural Yield Strength 108 MPa15700 psiBending Strength; ASTM D790
Flexural Modulus 3.10 GPa450 ksiBending Elasticity; ASTM D790
Izod Impact, Notched 0.640 J/cm1.20 ft-lb/inASTM D256
Taber Abrasion, mg/1000 Cycles 2.02.0ASTM D1175
Film Tensile Strength at Break, MD 59.0 MPa8560 psiOrientation not specified; ASTM D882
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 5.45.4Frequency Not Specified
Dissipation Factor 0.220.22Frequency Not Specified
 
Thermal PropertiesMetricEnglishComments
CTE, linear 70.0 µm/m-°C38.9 µin/in-°FBelow Tg
 120 µm/m-°C66.7 µin/in-°FAbove Tg
Specific Heat Capacity 2.40 J/g-°C0.574 BTU/lb-°F
Thermal Conductivity 0.340 W/m-K2.36 BTU-in/hr-ft²-°FFor EVAL F101
Melting Point 175 °C347 °FDSC
Deflection Temperature at 0.46 MPa (66 psi) 90.0 °C194 °F
Vicat Softening Point 165 °C329 °F
Glass Transition Temp, Tg 62.0 °C144 °FDynamic Viscoelasticity
 
Optical PropertiesMetricEnglishComments
Haze 1.5 %1.5 %Film; ASTM D1003
Gloss 90 %90 %45°; Film; ASTM D2457
 
Processing PropertiesMetricEnglishComments
Melt Temperature <= 240 °C<= 464 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema Evatane® 1020 VN 3 Ethylene Vinyl Acetate
EVALCA EVAL® LC-T101 Ethylene Vinyl Alcohol Copolymer Resin
EVALCA EVAL® LC-L101A Ethylene Vinyl Alcohol Copolymer Resin
EVALCA EVAL® LC-F101BZ Ethylene Vinyl Alcohol Copolymer Resin
EVALCA EVAL® F100 Ethylene Vinyl Alcohol Copolymer Resin

PEVAL6 / 37296

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.