MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

ATI Wah Chang Zirconium Alloy Zircaloy-4
Categories: Metal; Nonferrous Metal; Zirconium Alloy

Material Notes: Zirconium resists corrosive attack in most organic and mineral acids, strong alkalis, and some molten salts. A tightly adherent and protective oxide film protects the metal-oxide interface to provide corrosion resistance. An additional benefit for zirconium alloys in long-term geological disposal options is the inert nature of zirconium oxide.

Information provided by ATI Wah Chang

Key Words: UNS R60804
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 6.56 g/cc0.237 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 8989
Tensile Strength, Ultimate  241 MPa
@Temperature 288 °C
34900 psi
@Temperature 550 °F
Transverse
 271 MPa
@Temperature 288 °C
39300 psi
@Temperature 550 °F
Longitudinal
 514 MPa
@Temperature 23.0 °C
74600 psi
@Temperature 73.4 °F
 541 MPa
@Temperature 23.0 °C
78400 psi
@Temperature 73.4 °F
Tensile Strength, Yield  152 MPa
@Temperature 288 °C
22000 psi
@Temperature 550 °F
Longitudinal
 177 MPa
@Temperature 288 °C
25600 psi
@Temperature 550 °F
Transverse
 381 MPa
@Temperature 23.0 °C
55200 psi
@Temperature 73.4 °F
 467 MPa
@Temperature 23.0 °C
67800 psi
@Temperature 73.4 °F
Modulus of Elasticity 99.3 GPa14400 ksi
Poissons Ratio 0.370.37
Shear Modulus 36.19 GPa5249 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 6.00 µm/m-°C
@Temperature 20.0 °C
3.33 µin/in-°F
@Temperature 68.0 °F
Thermal Conductivity 21.5 W/m-K149 BTU-in/hr-ft²-°F
Melting Point 1850 °C3360 °F
 
Component Elements PropertiesMetricEnglishComments
Chromium, Cr 0.070 - 0.13 %0.070 - 0.13 %
Fe + Cr 0.28 - 0.37 %0.28 - 0.37 %
Iron, Fe 0.18 - 0.24 %0.18 - 0.24 %
Tin, Sn 1.2 - 1.7 %1.2 - 1.7 %
Zirconium, Zr 97.56 - 98.27 %97.56 - 98.27 %
 
Descriptive Properties
Alpha + Beta -> Beta Phase Transformation980°C
Alpha -> Alpha + Beta Phase Transformation810°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zircaloy-4 Zirconium Alloy
Zircaloy-2 Zirconium Alloy
Grade 706 Zirconium (Zr-2.5Nb)
Reactor Grade Zirconium
Zr-2.5Nb Zirconium Alloy, Nuclear Grade

NATIWC20 / 15075

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.