Celanese Impet® Hi430 15% Glass Filled, Impact Modified PET
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polyethylene Terephthalate (PET)
;
Polyethylene Terephthalate (PET), 30% Glass Reinforced
Material Notes:
Description:
Impet Hi 430 is a 15% glass filled and impact modified PET which has an excellent balance of mechanical properties as well as excellent processability and surface appearance.
Information provided by Celanese Corporation.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.33
g/cc
0.0480
lb/in³
ISO 1183 & ASTM D792
Linear Mold Shrinkage
0.0020
-
0.0050
cm/cm
0.0020
-
0.0050
in/in
ASTM D955
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
67.6
MPa
9800
psi
ASTM D638
73.0
MPa
10600
psi
5 mm/min; ISO 527-2/1A
Elongation at Break
3.0 %
3.0 %
5 mm/min; ISO 527-2/1A
Tensile Modulus
4.27
GPa
620
ksi
ASTM D638
4.80
GPa
696
ksi
1 mm/min; ISO 527-2/1A
Flexural Strength
115
MPa
16700
psi
ISO 178
Flexural Yield Strength
110
MPa
16000
psi
ASTM D790
Flexural Modulus
3.65
GPa
530
ksi
ASTM D790
4.20
GPa
609
ksi
ISO 178
Izod Impact, Notched
1.82
J/cm
3.40
ft-lb/in
ASTM D256
Izod Impact, Notched (ISO)
18.0
kJ/m²
8.57
ft-lb/in²
ISO 180/1A
Izod Impact, Unnotched (ISO)
30.0
kJ/m²
14.3
ft-lb/in²
ISO 180/1U
Charpy Impact Unnotched
5.30
J/cm²
25.2
ft-lb/in²
ISO 179/1eU
3.80
J/cm²
@Temperature -30.0 °C
18.1
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched
1.60
J/cm²
7.61
ft-lb/in²
ISO 179/1eA
0.840
J/cm²
@Temperature -30.0 °C
4.00
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
Electrical Properties
Metric
English
Comments
Dielectric Strength
19.3
kV/mm
490
kV/in
Short Term; ASTM D149
Arc Resistance
120
sec
120
sec
ASTM D495
Comparative Tracking Index
400
V
400
V
ASTM D3638
Thermal Properties
Metric
English
Comments
CTE, linear
30.0
µm/m-°C
@Temperature 20.0 °C
16.7
µin/in-°F
@Temperature 68.0 °F
ISO 11359-2
Melting Point
250
°C
482
°F
ISO 11357-1,2,3
Deflection Temperature at 0.46 MPa (66 psi)
223
°C
433
°F
ASTM D648
236
°C
457
°F
ISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi)
141
°C
286
°F
ISO 75-1, -2
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
260
-
270
°C
500
-
518
°F
Middle Barrel Temperature
270
-
280
°C
518
-
536
°F
Front Barrel Temperature
280
-
285
°C
536
-
545
°F
Nozzle Temperature
270
-
290
°C
518
-
554
°F
Melt Temperature
270
-
290
°C
518
-
554
°F
Mold Temperature
130
°C
266
°F
Back Pressure
0.552
MPa
80.0
psi
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Hippe PET Polyethylene Terephthalate
GEHR Plastics PET Polyethylene Terephthalate
Indorama AlphaPet Preformance® 1708CC(A) PET Resin
Indorama AlphaPet Preformance® 1708HS(A) PET Resin
Indorama Auriga Polymers Invista™ Polyclear™ Crystal™ 3302 PET Resin
PHCW57 / 45998
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.