  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Celanese Celanex® 602AC PBT, Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass Filled, Impact Modified

Material Notes: Celanex 602AC is a 10% fiberglass reinforced PBT that has lower warpage and improved impact over standard PBT.
To avoid hydrolytic degradation during processing, CELANEX resins have to be dried to a moisture level equal to or less than 0.02%. Drying should be done in a dehumidifying hopper dryer capable of dewpoints <-40°F (-40°C) at 250°F (121°C) for 4 hours.
For subsequent storage of the material in the dryer until processed (<= 60 h) it is necessary to lower the temperature to 100° C.

Information provided by Celanese Corporation.

Key Words: 10% Glass reinforced, low warp. improved impact
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.29 g/cc1.29 g/ccASTM D792
Density 1.29 g/cc0.0466 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inASTM D955
 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0060 - 0.0090 cm/cm0.0060 - 0.0090 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 83.0 MPa12000 psi5mm/min; ISO 527-2/1A
 65.5 MPa
@Temperature 22.8 °C
9500 psi
@Temperature 73.0 °F
ASTM D638
Elongation at Break 3.5 %3.5 %5mm/min; ISO 527-2/1A
 5.0 %
@Temperature 22.8 °C
5.0 %
@Temperature 73.0 °F
ASTM D638
Tensile Modulus 4.48 GPa
@Temperature 22.8 °C
650 ksi
@Temperature 73.0 °F
ASTM D638
Flexural Strength 120 MPa17400 psiISO 178
 111 MPa
@Temperature 22.8 °C
16100 psi
@Temperature 73.0 °F
ASTM D790
Flexural Modulus 4.23 GPa614 ksiISO 178
 3.59 GPa
@Temperature 22.8 °C
520 ksi
@Temperature 73.0 °F
ASTM D790
Izod Impact, Notched 0.694 J/cm
@Temperature 22.8 °C
1.30 ft-lb/in
@Temperature 73.0 °F
ASTM D256
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²ISO 180/1A
Izod Impact, Unnotched (ISO) 40.0 kJ/m²
@Temperature 23.0 °C
19.0 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.20e+17 ohm-cm1.20e+17 ohm-cmASTM D257
Dielectric Constant 3.4
@Frequency 1e+6 Hz
3.4
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 16.5 kV/mm420 kV/inshort term; ASTM D149
Dissipation Factor 0.017
@Frequency 1e+6 Hz
0.017
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 129 sec129 secASTM D495
 
Thermal PropertiesMetricEnglishComments
Melting Point 225 °C437 °FISO 11357-1,-2,-3; ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 202 °C396 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 139 °C282 °FISO 75-1, -2
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 50.0 °C68.0 - 122 °Fhopper
 65.0 - 93.0 °C149 - 199 °Fcavity
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 250 - 260 °C482 - 500 °F
Melt Temperature 235 - 260 °C455 - 500 °F
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4 hour4 hour
Moisture Content 0.020 %0.020 %Necessary low maximum
Hot-Working Temperature 250 - 260 °C482 - 500 °F
 
Descriptive Properties
Injection speedmedium-fast

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCS084 / 123499

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.