MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Crucible Steel KETOS® Tool Steel, AISI O1
Categories: Metal; Ferrous Metal; Tool Steel; Oil-Hardening Steel

Material Notes: Ketos is an oil-hardening tool steel which may be hardened from fairly low temperatures with little size change. This grade combines deep-hardening qualities with a fine-grained structure, affording good initial production runs, and good continued production after grinding.

Information provided by Crucible Industries

Key Words: AISI O1
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.83 g/cc0.283 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 187 - 221187 - 221
Hardness, Rockwell C 63 - 6563 - 65hardened at 1475°F then quenched
 39 - 41
@Tempering Temp. 538 °C
39 - 41
@Tempering Temp. 1000 °F
hardened at 1475F then tempered
 43 - 45
@Tempering Temp. 482 °C
43 - 45
@Tempering Temp. 900 °F
hardened at 1475F then tempered
 48 - 50
@Tempering Temp. 427 °C
48 - 50
@Tempering Temp. 800 °F
hardened at 1475F then tempered
 51 - 53
@Tempering Temp. 371 °C
51 - 53
@Tempering Temp. 700 °F
hardened at 1475F then tempered
 55 - 57
@Tempering Temp. 316 °C
55 - 57
@Tempering Temp. 600 °F
hardened at 1475F then tempered
 58 - 60
@Tempering Temp. 260 °C
58 - 60
@Tempering Temp. 500 °F
hardened at 1475F then tempered
 60 - 62
@Tempering Temp. 232 °C
60 - 62
@Tempering Temp. 450 °F
hardened at 1475F then tempered
 61 - 63
@Tempering Temp. 204 °C
61 - 63
@Tempering Temp. 400 °F
hardened at 1475F then tempered
 62 - 64
@Tempering Temp. 177 °C
62 - 64
@Tempering Temp. 350 °F
hardened at 1475F then tempered
 63 - 65
@Tempering Temp. 149 °C
63 - 65
@Tempering Temp. 300 °F
hardened at 1475F then tempered
Modulus of Elasticity 207 GPa30000 ksi
Charpy Impact  19.0 J
@Tempering Temp. 149 °C
14.0 ft-lb
@Tempering Temp. 300 °F
hardened at 1475°F then tempered; C-notch
 38.0 J
@Tempering Temp. 177 °C
28.0 ft-lb
@Tempering Temp. 350 °F
hardened at 1475°F then tempered; C-notch
 40.7 J
@Tempering Temp. 204 °C
30.0 ft-lb
@Tempering Temp. 400 °F
hardened at 1475°F then tempered; C-notch
 40.7 J
@Tempering Temp. 260 °C
30.0 ft-lb
@Tempering Temp. 500 °F
hardened at 1475°F then tempered; C-notch
 43.4 J
@Tempering Temp. 316 °C
32.0 ft-lb
@Tempering Temp. 600 °F
hardened at 1475°F then tempered; C-notch
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.6 µm/m-°C
@Temperature 21.1 - 204 °C
7.00 µin/in-°F
@Temperature 70.0 - 400 °F
 13.3 µm/m-°C
@Temperature 21.1 - 427 °C
7.40 µin/in-°F
@Temperature 70.0 - 800 °F
 14.0 µm/m-°C
@Temperature 21.1 - 538 °C
7.80 µin/in-°F
@Temperature 70.0 - 1000 °F
Thermal Conductivity 34.5 W/m-K
@Temperature 95.0 °C
239 BTU-in/hr-ft²-°F
@Temperature 203 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 743 °C1370 °FCritical Thermal Treatment Temperature
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.90 %0.90 %
Chromium, Cr 0.50 %0.50 %
Iron, Fe 96.55 %96.55 %as balance
Manganese, Mn 1.25 %1.25 %
Silicon, Si 0.30 %0.30 %
Tungsten, W 0.50 %0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bohler-Uddeholm O1 Cold Work Tool Steel
AISI Type O1 Oil-hardening Tool Steel, oil quenched at 800°C, tempered at 425°C
Latrobe LSS™ O1 Tool Steel (ASTM O1)
AISI 1045 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round
Crucible Steel HALGRAPH® Tool Steel, AISI O6

NCRUC913 / 160364

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.