MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Kleerdex Vinyloy™ 102 Acrylic/PVC Thermoplastic Sheet  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Acrylic (PMMA); Vinyl (PVC); PVC/Acrylic Alloy

Material Notes: Recycled capped FR sheet

Applications: Vinyloy 102 sheet is capped sheet that can be used to substitute effectively for ABS and other grades of thermoplastic sheet for your thermoforming needs.

Features: It has high impact resistance, rigidity, and thermoformability. Various colors are available.

Fabrication: Excellent forming properties result in uniform wall thicknesses and crisp detail, plus easy machining and fabricating using conventional methods, further expanding finished part possibilities.

Data provided by the Kleerdex Company.

Kleerdex Company became KYDEX, LLC in 2009.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ASTM D792
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 8888ASTM D785
Tensile Strength, Ultimate 42.0 MPa6090 psiASTM D638
Modulus of Elasticity 2.068 GPa299.9 ksi
Flexural Yield Strength 63.0 MPa9140 psiASTM D790
Izod Impact, Notched 4.27 J/cm
@Temperature 23.0 °C
8.00 ft-lb/in
@Temperature 73.4 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 78.0 °C172 °Fannealed; ASTM D648
Flammability, UL94 V-0V-0V-0, 5V; UL Standard 94
 
Processing PropertiesMetricEnglishComments
Processing Temperature 162 - 200 °C324 - 392 °FForming Temperature

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SEKISUI SPI KYDEX® 5555 Acrylic/PVC
PolyMirae Moplen HP552R Fiber (Staple/BCF/CF) Grade Polypropylene
Celanese Hostaform® C 2521 LS POM, UV Resistant
Celanese Hostaform® AM90S POM, Specialty
Celanese Hostaform® AM90S Plus POM, Specialty

PKLEER23 / 48876

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.