MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Celanese Rynite® 830ER BK503 PET-IGF30
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), 30% Glass Reinforced

Material Notes: 30% Glass Reinforced, Polyethylene Terephthalate Developed for Encapsulation Applications

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.59 g/cc0.0574 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 170 MPa24700 psiISO 527-1/-2
Elongation at Break 2.2 %2.2 %ISO 527-1/-2
Tensile Modulus 11.0 GPa1600 ksiISO 527-1/-2
Poissons Ratio 0.340.34
Charpy Impact Unnotched 6.09 J/cm²
@Temperature 23.0 °C
29.0 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.990 J/cm²
@Temperature 23.0 °C
4.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+14 ohm1.00e+14 ohmIEC 62631-3-2
Dielectric Constant  3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.3
@Frequency 100 Hz
4.3
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 36.0 kV/mm914 kV/inIEC 60243-1
Dissipation Factor  0.0020
@Frequency 100 Hz
0.0020
@Frequency 100 Hz
IEC 62631-2-1
 0.0148
@Frequency 1e+6 Hz
0.0148
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 250 V250 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 250 °C482 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 247 °C477 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 225 °C437 °FISO 75-1/-2
Flammability, UL94  HB
@Thickness 0.850 mm
HB
@Thickness 0.0335 in
IEC 60695-11-10
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 285 °C545 °FOptimum, Injection
 280 - 300 °C536 - 572 °FRange, Injection
Mold Temperature 120 - 140 °C248 - 284 °FInjection
 140 °C284 °FOptimum, Injection
Ejection Temperature 170 °C338 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.020 %<= 0.020 %Injection
Hold Pressure >= 80.0 MPa>= 11600 psiInjection
 
Descriptive Properties
Back pressureAs low as possible
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>PET-IGF30<ISO 11469
PolymerPET-GF30
Processing Hold Pressure Time (s/mm)4Injection
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPET-IGF30ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDSX4843 / 256292

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.