MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Crucible Steel LABELLE® Silicon #2 Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel; Shock-Resisting Steel

Material Notes: LaBelle Silicon #2 is a shock resisting tool steel capable of maximum toughness at relatively high hardness. It has excellent resistance to impact and battering, with good edge retention.

Information provided by Crucible Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.75 g/cc0.280 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 187 - 235187 - 235
Hardness, Rockwell C 60 - 6160 - 61oil quenched from 1650°F
 64 - 6564 - 65water quenched from 1600°F
 44 - 45
@Tempering Temp. 538 °C
44 - 45
@Tempering Temp. 1000 °F
hardened at 1650°F then tempered
 47 - 48
@Tempering Temp. 482 °C
47 - 48
@Tempering Temp. 900 °F
hardened at 1650°F then tempered
 51 - 52
@Tempering Temp. 427 °C
51 - 52
@Tempering Temp. 800 °F
hardened at 1650°F then tempered
 56 - 57
@Tempering Temp. 371 °C
56 - 57
@Tempering Temp. 700 °F
hardened at 1650°F then tempered
 57 - 58
@Tempering Temp. 316 °C
57 - 58
@Tempering Temp. 600 °F
hardened at 1650°F then tempered
 58 - 59
@Tempering Temp. 260 °C
58 - 59
@Tempering Temp. 500 °F
hardened at 1650°F then tempered
 58 - 60
@Tempering Temp. 204 °C
58 - 60
@Tempering Temp. 400 °F
hardened at 1650°F then tempered
 60 - 61
@Tempering Temp. 149 °C
60 - 61
@Tempering Temp. 300 °F
hardened at 1650°F then tempered
Modulus of Elasticity 207 GPa30000 ksi
Charpy Impact  66.4 J
@Tempering Temp. 149 °C
49.0 ft-lb
@Tempering Temp. 300 °F
hardened at 1650°F then tempered; C-notch
 187 J
@Tempering Temp. 204 °C
138 ft-lb
@Tempering Temp. 400 °F
hardened at 1650°F then tempered; C-notch
 193 J
@Tempering Temp. 316 °C
142 ft-lb
@Tempering Temp. 600 °F
hardened at 1650°F then tempered; C-notch
 198 J
@Tempering Temp. 260 °C
146 ft-lb
@Tempering Temp. 500 °F
hardened at 1650°F then tempered; C-notch
 212 J
@Tempering Temp. 371 °C
156 ft-lb
@Tempering Temp. 700 °F
hardened at 1650°F then tempered; C-notch
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.6 µm/m-°C
@Temperature 21.1 - 427 °C
7.00 µin/in-°F
@Temperature 70.0 - 800 °F
 13.3 µm/m-°C
@Temperature 21.1 - 538 °C
7.40 µin/in-°F
@Temperature 70.0 - 1000 °F
 13.7 µm/m-°C
@Temperature 21.1 - 649 °C
7.60 µin/in-°F
@Temperature 70.0 - 1200 °F
Thermal Conductivity 33.0 W/m-K
@Temperature 95.0 °C
229 BTU-in/hr-ft²-°F
@Temperature 203 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 766 °C1410 °FCritical Thermal Treatment Temperature
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.60 %0.60 %
Chromium, Cr 0.25 %0.25 %
Iron, Fe 95.9 %95.9 %as balance
Manganese, Mn 0.85 %0.85 %
Molybdenum, Mo 0.30 %0.30 %
Silicon, Si 1.9 %1.9 %
Vanadium, V 0.20 %0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Shock-Resisting Steel
AISI Type S2 Tool Steel, austenitized 845°C (1550°F), brine quenched to 55 HRC
ATI Allegheny Ludlum S7 Tool Steel, UNS T41907
AISI Type S1 Tool Steel, quenched 955°C (1750°F), tempered 150°C (300°F)
EDRO #7 Shock Resistant S7 Tool Steel

NCRUC915 / 160366

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.