MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Plenco 2535 Phenolic, Granular, Compression Molded
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Novolac, Woodflour Filled

Material Notes: PLENCO 02535 is a general purpose, organic filled phenolic molding compound offering optimized cure characteristics and excellent electrical properties. Type ASTM 5948 CFG, and UL recognized under component file E40654. 02535 is available in black or brown color.

Information supplied by Plenco.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.600 g/cc0.0217 lb/in³ASTM D1895
Density 1.39 g/cc0.0502 lb/in³ASTM D792
Water Absorption 0.45 %0.45 %ASTM D570
Linear Mold Shrinkage 0.0035 cm/cm0.0035 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 9191ASTM D785
Tensile Strength, Ultimate 59.0 MPa8560 psiASTM D638
Elongation at Break 0.77 %0.77 %ASTM D638
Tensile Modulus 8.50 GPa1230 ksiASTM D638
Flexural Strength 96.0 MPa13900 psiASTM D790
Flexural Modulus 8.80 GPa1280 ksiASTM D790
Compressive Strength 217 MPa31500 psiASTM D695
Izod Impact, Notched 0.199 J/cm0.373 ft-lb/inASTM D256
Charpy Impact, Notched 0.193 J/cm²0.919 ft-lb/in²ASTM D256
Impact 130130J/m Drop Ball Impact; PLENCO
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.00e+12 ohm-cm6.00e+12 ohm-cmASTM D247
Dielectric Constant 4.64.6ASTM D150
Dielectric Strength 14.3 kV/mm363 kV/inShort Time; ASTM D149
Dissipation Factor 0.0380.038ASTM D150
Arc Resistance 103 sec103 secASTM D495
Comparative Tracking Index 150 V150 VASTM D3638
 
Thermal PropertiesMetricEnglishComments
CTE, linear 68.0 µm/m-°C
@Temperature 40.0 - 130 °C
37.8 µin/in-°F
@Temperature 104 - 266 °F
TMA; ASTM E831
Thermal Conductivity 0.370 W/m-K
@Temperature 100 °C
2.57 BTU-in/hr-ft²-°F
@Temperature 212 °F
ASTM E1461
Maximum Service Temperature, Air 196 °C385 °FHeat Resistance; ASTM D570D
Deflection Temperature at 1.8 MPa (264 psi) 173 °C343 °FASTM D648
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
Oxygen Index 25 %25 %ASTM D2863
Shrinkage 0.195 %0.195 %72 hr, 120ºC; ASTM D1299

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plenco 1501 Polyester, Briquette, Transfer Molded
Plenco 2571 Phenolic, Granular, Compression Molded
Plenco 2000 Phenolic, Granular, Compression Molded
Plenco 4485 Phenolic, Granular, Injection Molded
Plenco 1510 Polyester, Granular, Transfer Molded

PLEL48 / 50616

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.